Michigan Technological University Digital Commons @ Michigan Tech Dissertations, Master's Theses and Master's Reports - Open Dissertations, Master's Theses and Master's Reports 2013 Intergranular Corrosion and Stress Corrosion Cracking of Extruded AA6005A David James Seguin Michigan Technological University Copyright 2013 David James Seguin Recommended Citation Seguin, David James, "Intergranular Corrosion and Stress Corrosion Cracking of Extruded AA6005A", Dissertation, Michigan Technological University, 2013. http://digitalcommons.mtu.edu/etds/652 Follow this and additional works at: http://digitalcommons.mtu.edu/etds Part of the Materials Science and Engineering Commons
INTERGRANULAR CORROSION AND STRESS CORROSION CRACKING OF EXTRUDED AA6005A By Daniel James Seguin A DISSERTATION Submitted in partial fulfillment of the requirements for the degree of DOCTOR OF PHILOSOPHY In Materials Science and Engineering MICHIGAN TECHNOLOGICAL UNIVERSITY 2013 2013 Daniel James Seguin
This dissertation has been approved in partial fulfillment of the requirements for the Degree of DOCTOR OF PHILOSPHY in Materials Science and Engineering. Department of Materials Science and Engineering Dissertation Advisor: Calvin L. White. Committee Member: Stephen Hackney Committee Member: Mark Plichta Committee Member: Richard Dickson Department Chair: Stephen Kampe
Table of Contents List of Figures... v List of Tables... ix Abstract... x 1 Introduction and Motivation... 1 2 Background... 3 2.1 Aluminum Metallurgy... 3 2.2 Extrusion Metallurgy... 5 2.3 Corrosion of Aluminum and Aluminum Alloys... 7 2.4 Stress Corrosion Cracking... 18 3 Hypotheses and Literature Review... 25 3.1 IGC and SCC Susceptibility of AA6005A: Literature Review... 25 3.2 Mechanism of SCC in AA6005A: Literature Review... 27 4 Experimental Methods and Results... 30 4.1 Materials... 30 4.2 Electrochemical Behavior of AA6005A Extrusions... 31 4.2.1 Experimental Methods - Polarization Experiments... 32 4.2.2 Results and Discussion Polarization Experiments... 35 4.3 IGC of the Elongated Grain Structure in AA6005A... 44 4.3.1 Experimental Methods IGC of AA6005A... 44 4.3.2 Results and Discussion IGC of AA6005A... 45 iii
4.3.3 Effects of Diffusion on IGC Velocity... 58 4.4 Qualitative measurement of SCC in AA6005A Extrusions... 76 4.4.1 Experimental Methods - Qualitative SCC of AA6005A... 76 4.4.2 Results and Discussion - Qualitative SCC of AA6005A... 79 4.5 Quantitative measurement of SCC in AA6005A Extrusions... 84 4.5.1 Experimental Methods Quantitative SCC of AA6005A... 84 4.5.2 Results - Quantitative SCC of AA6005A... 91 4.5.3 Discussion of Quantitative SCC Analysis... 99 4.5.4 Effects of Stress Triaxiality and Local Electrochemical Reactions on Stress Corrosion Cracking of AA6005A-T6... 106 5 Summary... 120 6 Conclusions... 127 6.1 Conclusions... 127 6.1.1 Conclusions based on Primary Hypotheses... 127 6.1.2 Additional Conclusions... 128 7 References... 132 8 Appendix A... 137 9 Appendix B... 139 iv
List of Figures Figure 1:Typical grain structure of AA6005A extrusions... 6 Figure 2: Pourbaix diagram for pure aluminum... 11 Figure 3: Schematic polarization curve with Tafel analysis.... 13 Figure 4: Method for determining anodic Tafel behavior.... 14 Figure 5: Effect of cathode to anode area ratio... 16 Figure 6: Schematic polarization curves for an active-passive metal... 17 Figure 7: Typical relationship between SC crack growth and stress intensity... 20 Figure 8: Schematic of a hydrogen embrittlement of SCC... 22 Figure 9: Schematic of an anodic dissolution mechanism of SCC... 23 Figure 10: Definition of coordinate system used to describe specimens... 31 Figure 11: Sample configuration used in polarization experiments... 33 Figure 12: Experimental setup for conducting polarization measurements... 34 Figure 13: Effect of ph on the polarization behavior of AA6005A-T6... 36 Figure 14:Effect of ph on the corrosion potential of AA6005A-T6... 37 Figure 15: Representative Tafel analysis for AA6005A-T6... 39 Figure 16: Effect of solution ph on the corrosion current density of AA6005A-T6. 40 Figure 17: Effect of heat treatment on the polarization behavior of AA6005A... 41 Figure 18: Effect of a hydrogen recombination poison on the polarization behavior of AA6005A-T6... 43 v
Figure 19: Effect of age treatment on the mode of corrosion attack... 46 Figure 20: Core grain boundary microstructure of AA6005A-T4... 47 Figure 21: Core grain boundary microstructure of AA6005A-T6... 48 Figure 22: Core grain boundary microstructure of AA6005A-OA... 49 Figure 23: Effect of ph on the severity of IGC in AA6005A-T6... 51 Figure 24: Typical anisotropic IGC attack observed in the elongated grain structure of AA6005A-T4... 52 Figure 25: Maximum observed depth of IGC attack in the elongated grain structure for AA6005A-T4.... 52 Figure 26: Maximum observed depth of IGC attack in the elongated grain structure for AA6005A-T6.... 53 Figure 27: (200) X-Ray pole figure of elongated grain structure in AA6005A... 55 Figure 28: Three-dimensional geometric model used to describe the anisotropic corrosion attack in the elongated grain structure of AA6005A extrusions... 56 Figure 29: Structure corrected corrosion path length for AA6005A-T6... 60 Figure 30: Structure corrected IGC velocity in AA6005A-T6... 61 Figure 31: Sample configuration used to qualitatively determine the variation in ph with corrosion depth... 63 Figure 32: Variation in ph within a simulated corrosion path.... 64 Figure 33: Sample configuration used to determine the local ph at varied IGC path lengths.... 66 vi
Figure 34: Effect of corrosion path length and acidity of bulk environment on the ph of the local environment within a simulated corrosion path... 67 Figure 35: Model of IGC path used to determine IGC velocity... 72 Figure 36: Test of diffusion-based model to predict IGC velocity in AA6005A-T6. 74 Figure 37: Modified sub-sized tensile bar geometry used for BLT.... 77 Figure 38: Experimental setup for conducting breaking load tests... 78 Figure 39: System for conducting qualitative SCC analysis of AA6005A... 79 Figure 40: Effect of heat treatment on the residual strength of AA6005A... 81 Figure 41: Effect of ph on SCC susceptibility in AA6005A-T6... 82 Figure 42: Effect of a hydrogen recombination poison on SCC susceptibility of AA6005A-T6... 83 Figure 43: Sample geometry of CT specimens used for crack growth rate measurements... 86 Figure 44: Modulus vs. crack length calibration of the sample configuration used in this work... 88 Figure 45: Schematic of setup that was used for SCC-CGR experiments... 89 Figure 46: Results from CGR experiment of AA7475 sheet e... 90 Figure 47: Crack growth rate of AA6005A-T6 extrusions... 92 Figure 48: Typical SEM micgrograph of AA6005A-T6 fracture surface after conducting SCC testing... 93 Figure 49: SEM micrograph of fracture surface within elongated grain structure of AA6005A-T6... 94 vii
Figure 50: Morphology of advancing crack in AA6005A-T6... 96 Figure 51: Effect of a hydrogen recombination poison (As2O3) on the crack growth rate of AA6005A-T6... 97 Figure 52: Fracture surface of AA6005A-T6 CGR specimen exposed to a solution of 3.5% NaCl + 0.3% As2O3 at ph = 1.5... 99 Figure 53: Structure-corrected corrosion velocity with increasing corrosion depth along direction 1 for stressed and unstressed samples.... 101 Figure 54: Effective corrosion path lengths along direction 2 for stressed SCC-CGR specimens with crack lengths greater than the 1/2 thickness of the sample... 103 Figure 55: Calculated velocity profile along the crack front of a CT sample... 105 Figure 56: Effect of plastic zone size on the stress state in a material.... 107 Figure 57: Crack morphology at various depths in a compact tensile bar of AA6005A-T6... 109 Figure 58: Schematic representation of the Nabarro-Herring model... 111 Figure 59: Local environment within a SC crack in a loaded CT specimen... 114 Figure 60: Predicted polarization behavior at a stress corrosion crack tip for AA6005A-T6 exposed to 3.5% NaCl at ph = 1.50.... 115 Figure 61: Predicted polarization behavior at a stress corrosion crack tip for AA6005A-T6 exposed to 3.5% NaCl at ph = 2.0.... 117 Figure 62: Structure corrected corrosion velocity for loaded CT samples of AA6005A-T6 exposed to 3.5% NaCl at ph=1.5 or ph=2.0... 119 viii
List of Tables Table 1: Primary alloying elements in wrought aluminum alloys... 3 Table 2: Precipitation sequence for solutionized 6xxx alloys... 4 Table 3: Composition specification for AA6005A alloy... 5 Table 4: Composition of AA6005A extrusions used in experiments... 30 Table 5: Yield and tensile stresses for AA6005A extrusions with varied heat treatment.... 30 Table 6: Calculated corrosion path lengths along all directions for samples in a T4 and T6 temper... 57 Table 7: Solubility products for several solid species that may control the ph within an IGC path in AA6005A-T6 [68]... 70 Table 8: Summary of electrochemical analysis for CT specimens exposed to ph =1.5, and ph =2.0 aerated saltwater solutions with and without an externally applied load.... 117 ix
Abstract A research program focused on understanding the intergranular corrosion (IGC) and stress corrosion cracking (SCC) behavior of AA6005A aluminum extrusions is presented in this dissertation. The relationship between IGC and SCC susceptibility and the mechanisms of SCC in AA6005A extrusions were studied by examining two primary hypotheses. IGC susceptibility of the elongated grain structure in AA6005A exposed to low-ph saltwater was found to depend primarily on the morphology of Cu-containing precipitates adjacent to the grain boundaries in the elongated grain structure. IGC susceptibility was observed when a continuous (or semi-continuous) film of Cucontaining phase was present along the grain boundaries. When this film coarsened to form discrete Cu-rich precipitates, no IGC was observed. The morphology of the Curich phase depended on post-extrusion heat treatment. The rate of IGC penetration in the elongated grain structure of AA6005A-T4 and AA6005A-T6 extrusions was found to be anisotropic with IGC propagating most rapidly along the extrusion direction, and least rapidly along the through thickness direction. A simple 3-dimensional geometric model of the elongated grain structure was accurately described the observed IGC anisotropy, therefore it was concluded that the anisotropic IGC susceptibility in the elongated grain structure was primarily due to geometric elongation of the grains. x
The velocity of IGC penetration along all directions in AA6005A-T6 decreased with exposure time. Characterization of the local environment within simulated corrosion paths revealed that a ph gradient existed between the tip of the IGC path and the external environment. Knowledge of the local environment within an IGC path allowed development of a simple model based on Fick s first law that considered diffusion of Al 3+ away from the tip of the IGC path. The predicted IGC velocity agreed well with the observed IGC velocity, therefore it was determined that diffusion of Al 3+ was the primary factor in limiting IGC velocity. The velocity of crack growth in compact tensile (CT) specimens of AA6005A-T6 extrusion exposed to 3.5% NaCl at ph = 1.5 was nearly constant over a range of applied stress intensities, exposure times, and crack lengths. The crack growth behavior oxf CT specimens of AA6005A-T6 extrusion exposed to a solution of 3.5% NaCl at ph = 2.0 exhibited similar behavior, but the crack velocity was ~10.5X smaller than that those exposed to a solution at ph =1.5. Analysis of the local stress state and polarization behavior at the crack tip predicted that increasing the ph of the bulk solution from 1.5 to 2.0 would decrease the corrosion current density at the crack tip by approximately 11.8X. This predicted decrease in corrosion current density was in reasonable agreement with the observed decrease in SCC velocity associated with increasing the solution ph from 1.5 to 2.0. The agreement between the predicted and observed SCC velocities suggested that the electrochemical reactions controlling SCC in AA6005A-T6 extrusions are ultimately controlled by the ph gradient that exists between the crack tip and external environment. xi
1 Introduction and Motivation Extruded Aluminum is among the most versatile engineering materials available today. Its high strength-to-weight ratio, relatively low associated cost, formability, and recyclability have made aluminum alloys appealing materials for use in a broad range of applications. The ability to manufacture elongated sections with complex two-dimensional profiles makes extrusion an efficient processing route for structural components from aluminum alloys. Extruded aluminum alloys have been used as the primary construction material in many advanced structures including solar power plant frames and aerospace fuselages. To fully realize the range of potential applications of aluminum extrusions as structural components, it is essential to understand how the material will behave in corrosive service environments, such as an industrial marine environment. The research discussed in this dissertation is focused on understanding fundamental mechanisms of intergranular corrosion (IGC) and stress corrosion cracking (SCC) of extruded AA6005A alloy in simulated marine environments. The original purpose of the research was to determine if IGC or SCC of AA6005A extrusions should be a major design consideration if there material were to be used in concentrated solar power plant (CSPP) frames in regions with a marine climate, such as Florida. The design lifetime for the CSPP frames was to be 30 years. 1
The specifications of the CSPP frames indicated that the extruded members of AA6005A would see a maximum tensile load of approximately 44 MPa (18% y), and maximum compressive load of approximately 46 MPa in severe (hurricane) conditions. These design values served as a baseline for beginning the study of IGC and SCC of AA6005A, and were used to assess the viability of the material for use in the CSPP frames. 2
2 Background 2.1 Aluminum Metallurgy There are eight general classes of wrought aluminum alloys recognized by the Aluminum Association (AA). Each series is defined by primary alloying element(s) that are added to achieve desired properties of the final product (Table 1). Specific alloy designations within each class are defined by concentrations of primary and secondary alloying elements. The research presented here will focus on AA6005A extrusions. The primary alloying elements in AA6005A are Mg and Si. There is limited literature available on intergranular corrosion (IGC) and no literature on stress-corrosion cracking (SCC) of AA6005A. Much of the background data relevant to the research program is therefore focused on other 6xxx alloys. Relevant comparisons to other alloy classes, such as 2xxx and 7xxx, is also used to formulate hypotheses and propose research activities. Table 1: Primary alloying elements in wrought aluminum alloys Series 1xxx 2xxx 3xxx 4xxx 5xxx 6xxx 7xxx 8xxx Other Primary (Li, Alloying N/A Cu Mn Si Mg Si, Mg Zn Fe, Elements (etc.) The combination of strength, formability, and good corrosion resistance make these 6xxx commonly used materials in engineering applications. Mechanical strength of solution treated 6xxx alloys can be improved by precipitation hardening 3
(aging). Aging is generally done at intermediate temperatures (~185 C), but some degree of strengthening can be achieved by naturally aging the material for an extended period of time at room temperature. The primary strengthening phase of 6xxx alloys, Mg2Si (, is formed through a sequence of steps, as shown in Table 2 [1, 2]: Table 2: Precipitation sequence for solutionized 6xxx alloys Precipitate Structure 1 Saturated solid solution FCC solid solution 2 Solute rich Guinier Preston zones Clusters of solute species 3 Coherent (Mg5Si6) precipitates Monoclinic 4 Semi-coherent precipitates Structure unknown 5 Incoherent (Mg2Si) precipitates Cubic The first step in the precipitation sequence for 6xxx alloys is formation of small Guinier Preston (GP) zones. The GP zones combine to form coherent monoclinic Mg5Si6 ( ) precipitates upon thermal treatment. Further thermal treatment causes the phase to form semi-coherent precipitates. The structure and chemistry of is not well known, but it has been suggested that has a hexagonal structure, and forms rod-like precipitates [3]. The final step in the precipitation sequence involves the formation of, which is incoherent and has a cubic crystal structure. Optimal strength of 6xxx alloys is achieved with a dense, homogeneous network of fine precipitates in the material [1]. Adding Mg and Si in a near 5:6 molar ratio and using a well-controlled heat treatment process can promote precipitation of. The alloy AA6005A incorporates this Mg:Si molar ratio to yield a 4
near optimal medium strength wrought aluminum alloy. The AA composition specification for AA6005A alloy is given in Table 3. Because of this near-optimized composition, extruded AA6005A alloy is more easily formed and less quench sensitive than some of the other 6xxx alloys with similar mechanical strength specifications (e.g. AA6061). In addition to Mg and Si, the AA specification for AA6005A allows for up to 0.3 wt. % Cu. The Cu is added to improve the mechanical strength of the alloy through precipitation of certain strengthening phases. However, it has been demonstrated through a number of reports that Cu in excess of about 0.12 wt. % can make the alloy susceptible to IGC when the alloy has certain thermomechancial histories [4-8]. Table 3: Composition specification for AA6005A alloy Cr Cu Fe Mg Mn Si Ti Zn Other, each Other, total Al 0.40-0.70 0.50-0.90 Bal. 2.2 Extrusion Metallurgy Aluminum extrusion is a high-temperature deformation process in which elongated parts with a fixed cross sectional profile are manufactured by pressing a pre-heated billet through a precision die. This seemingly simple process is actually quite complex because extrusion is a non-steady-state process in which deformation mechanisms, heat generation, and friction evolve each extrusion cycle. There are several features characteristic of extruded profiles that are pertinent to the present study. 5
Extrusions of AA6005A alloy, as with many other extruded alloys, have a duplex grain structure consisting of an elongated grain structure in the core of the material, and an equiaxed layer near the surface as illustrated in Figure 1. The elongated structure in air quenched AA6005A contains fully recrystallized grains that are oriented along the extrusion direction. The equiaxed layer consists of randomly oriented grains which generally have higher angle boundaries than those found in the elongated core structure [9]. A thick recrystallized layer is known to be detrimental to the mechanical performance of the final product [10]. Studies have also shown that an equiaxed grain structure may be more susceptible to IGC than an elongated structure in extruded Al alloys [9]. Limiting the degree of deformation during extrusion, and achieving a rapid quench after extrusion can minimize the thickness of the equiaxed layer [11]. Figure 1:Typical grain structure of AA6005A extrusions consisting of equiaxed grains near the extrusion surface (top of micrograph), and elongated grains (near bottom of micrograph) in the core of the extrusion. Direction 1 is the extrusion direction, and direction 2 is the through thickness direction. 6
The elongated grain structure in aluminum extrusions can give rise to anisotropic mechanical properties and anisotropic corrosion behavior [11, 12]. The origin of the anisotropic corrosion behavior in the elongated structure of wrought aluminum alloys has been extensively reported [12-16]. Researchers have determined that texture and grain boundary misorientation angle can have a dramatic effect on the grain boundary precipitate structure in wrought aluminum alloys, thereby giving rise to anisotropic IGC [9, 12]. In many cases, anisotropic IGC has been simply attributed to geometric anisotropy of the grains providing a less tortuous path for corrosion attack along the deformation direction [15-17]. Zhang et al. studied the relationship between grain elongation and preferential attack along the extrusion direction in AA2024-T3 plate [15]. Zhang modeled the anisotropic grain structure as a two-dimensional brick wall with the edge lengths of the bricks corresponding to the nominal grain size along each direction. Zhang quantitatively predict the anisotropic corrosion attack in the anisotropic grain structure using this simple geometric configuration, and considering the density of initiation sites along different surfaces in the material. Several studies have used models similar to Zhang s to describe anisotropic corrosion attack in wrought aluminum alloys [12, 14-17]. 2.3 Corrosion of Aluminum and Aluminum Alloys Corrosion is the degradation of a material due to electrochemical interactions with the service environment. There are two fundamental chemical reactions that 7
control all corrosion processes in metallic systems. The first is the anodic (oxidation) reaction in which metal ions are dissociated from the parent alloy, leaving behind free electrons (Equation 1). Electrons created by the anodic reaction are conducted through the metal to participate in the cathodic (reduction) reaction, sometimes at a significant distance from the location of the anodic reaction. The cathodic reaction involves species from the environment (typically ionic) consuming the electrons that are produced at the site of the anodic reaction. The most common cathodic reaction in acidic environments involves reduction of H + ions to form H2 gas (Equation 2) [18]. The electrochemical driving force for corrosion reactions is the difference in the halfcell potentials (E) for the anodic and cathodic reactions. The standard state half-cell potentials for each of the reactions are given below. Equation 1 [19] Equation 2 [19] = +3 2 +2 = = 1.66 =0 The H2 evolution reaction (Equation 2) occurs in three distinct steps [18]. First, H + reacts with an electron from the metal surface to form an adsorbed H atom (Hads) at the metal surface (Equation 3). The Hads then combines with another Hads to form an adsorbed hydrogen molecule (H2ads) (Equation 4). The H2ads molecules then combine to form an H2 bubble at the metal surface. Adding a hydrogen recombination poison, such as As 3+, to the electrolyte tends to inhibit the recombination of Hads, thereby increasing the concentration of atomic H in the material [20, 21]. 8
Equation 3 [18] Equation 4 [18] + = 2 = The effects of temperature and concentration of ionic species on the half-cell corrosion potentials of the reactions listed above can be determined using the Nernst equation (Equation 5) [18, 19]. The standard form of the Nernst equation is: Equation 5 = ln Where E is the half-cell corrosion potential for a reaction, E o is the half-cell corrosion potential for a reaction when all reactants and products are in their standard states, R is the ideal gas constant, T is the absolute temperature of the reaction, n is the number of electrons involved in the half cell reaction, F is Faraday s constant (96,500 C/mol), and ax x is the activity of specific species involved in the half cell reaction. The activities of the products of the reaction are in the numerator of in Equation 5, and the activities of the reactants are in the denominator. The activity of a dissolved species is usually assumed to be equal to its concentration, and the activity of a pure solid or gas at atmospheric pressure is unity. The exponents in Equation 5 are the stoichiometric coefficients of the corresponding elements in the half-cell reactions. Aluminum is an electrochemically active metal, but is generally regarded as having good corrosion resistance due to the rapid formation of a passive oxide film on the metal surface. The passive film consists of two layers: 1) A continuous 9
amorphous oxide film adjacent to the parent metal and 2) A porous crystalline layer between the amorphous layer and the external environment [22]. The passive layer, which has the approximate composition of Al2O3, acts as a kinetic barrier that slows dissolution of the corroding material. Discontinuities in the Al2O3 film often serve as initiation sites for localized corrosion in Al alloys [23]. A Pourbaix diagram illustrates the range of ph and electrochemical potential in which an Al2O3 passive layer is thermodynamically stable on pure aluminum (Figure 2). It is evident from the Pourbaix diagram that the passive layer on aluminum becomes unstable in acidic or alkaline environments when at higher applied potential [19]. The range of ph and potential in which the passive layer is stable depends on the concentration of the corrosion product (either Al 3+ or AlO2 - ) in solution. The values of ph at which given concentrations of Al 3+ and AlO2 - are in equilibrium with the passive layer are determined using the Nernst equation. The vertical lines located on the upper left side of the Pourbaix diagram correspond to conditions in which Al2O3 and Al 3+ are in thermodynamic equilibrium. These vertical lines are key features of the Pourbaix diagram that will be used to develop a model to describe IGC penetration later in the dissertation. 10
Figure 2: Pourbaix diagram for pure aluminum. The stability of the Al2O3 depends on the applied potential, ph, and the concentration of corrosion product. The corrosion rate and corrosion potential of a material in specific environments may be characterized by conducting polarization measurements. Polarization measurements are performed by applying a range of known electrochemical potentials to a sample and measuring the resulting corrosion current density. The output of a polarization measurement is a single curve that contains information about both the cathodic and anodic reactions involved in a specific corrosion reaction. It is important to note that the observed polarization curves actually reflect the electrochemical response of the electrolytic solution adjacent to the surface of the sample. 11
The polarization behavior of a corrosion reaction depends not only on the equilibrium electrochemical properties of the anodic and cathodic reactions, but also on kinetic properties of the reactions. The exchange current density (io) of a half-cell reaction is a characteristic value that defines the kinetics of that reaction under equilibrium conditions. Changes in ionic concentration and temperature can shift the value of io to higher or lower values, thereby altering the observed polarization behavior of a corrosion reaction. The kinetics of a reaction may also depend on both the surface properties of the alloy. For example, the rate of cathodic and anodic reactions may be slowed by the presence of a passive layer on the surface of the corroding metal due to poor electrical conductivity of the passive layer [24]. This would tend to shift the exchange current density of the cathodic reaction to a lower value, thereby changing the observed values of corrosion potential (ECorr) and corrosion current density (icorr). Values of corrosion current density are extracted from polarization curves by performing Tafel analysis [18, 19, 25]. A simple example of a Tafel analysis is illustrated in Figure 3. The solid line illustrates the overall polarization response of the material, and the dashed lines illustrate the Tafel curves for the anodic and cathodic reactions. Tafel analysis involves extrapolating a region of linear V vs. log(i) behavior in the anodic and cathodic portions of the polarization curve. When the slope of the V vs. log(i) is near linear, the reaction rate is controlled by activation polarization. Activation polarization occurs when the observed polarization behavior of the electrochemical reaction reflects the activation energy for electron transfer 12
between the electrolyte and electrode (sample) [19]. The slope of each of the curves is the Tafel constant,. The intersection of the anodic and cathodic Tafel curves corresponds to the corrosion current density, icorr, for a given corrosion reaction. Figure 3: Schematic polarization curve with Tafel analysis. In practice, Tafel analysis of the anodic portion of a polarization curve is often more difficult than the situation illustrated in Figure 3 because there is rarely a significant linear region in the anodic portion of the V vs. log(i) curve. A technique summarized by Jones can be used to perform Tafel analysis of the anodic portion of a polarization curve [19]. Jones technique is performed by first determining a region of Tafel behavior in the cathodic portion of a polarization curve. A series of points at 13
values of electrochemical potential above the region of linearity in the cathodic curve (indicated by hollow circles in Figure 4) are then selected. The values of corrosion current density at these points (iexp) are subtracted from values of corrosion current density on the cathodic Tafel curve (ic) to determine the anodic corrosion current density (ia, indicated by the filled circles in Figure 4) at values of electrochemical potential below the open circuit corrosion potential. An anodic Tafel curve is then generated by extrapolating the calculated values of ia to higher electrochemical potentials. Figure 4: Method for determining anodic Tafel behavior. The relative surface areas on which anodic and cathodic reactions are occurring can have a significant influence on the overall kinetics of a corrosion 14
reaction [19]. This concept is schematically illustrated with Tafel plots in Figure 5. First consider a corrosion reaction in which the cathode to anode area ratio is 1:1. Assume the exchange current density of the anodic reaction is ioa, and the exchange current density of the cathodic reaction is ioc1 in this case. The resulting corrosion current density in this case would be icorr1. Now consider a case in which the cathodic surface area is increased by 100X and the anodic surface area is held constant. Increasing the cathodic surface area would increase the exchange current density of the cathodic reaction, causing the cathodic Tafel curve to intersect the anodic Tafel curve at a higher value of current density and corrosion potential. The resulting corrosion current density would therefore be increased to icorr2. 15
Figure 5: Effect of cathode to anode area ratio on the kinetics of a corrosion reaction. Schematic anodic and cathodic polarization curves for a metal exhibiting active-passive behavior (e.g. aluminum) are illustrated as dashed lines in Figure 6. The experimentally observed current density (solid black lines) of the alloy is the algebraic sum of the cathodic and anodic polarization current, represented by dashed lines in Figure 6. The regions of active, passive, and transpassive behavior are indicated in Figure 6A. The point at which the anodic and cathodic reactions intersect corresponds to the characteristic corrosion rate (measured corrosion current density, icorr ) and open circuit corrosion potential, ECorr, of the reaction. If the cathodic polarization curve intersects the anodic polarization curve reaction at a potential 16
corresponding to passive behavior (as shown in Figure 6A), the corrosion rate is limited by the presence of a passive film, and is relatively low. If the cathodic reaction is shifted such that it intersects the transpassive region in the anodic polarization curve, as shown in Figure 6B, the passive layer is not stable, and the resulting corrosion rate is larger. A cathodic reaction in an acidic environment can be shifted up or down by changing the ph of the solution, or changing the partial pressure of gases involved in the cathodic reaction [18]. Figure 6: Schematic polarization curves for a metal exhibiting active-passive behavior. The dashed lines illustrate the cathodic and anodic reactions, and the bold solid lines illustrate the observed polarization behavior. If the cathodic and anodic reactions intersect at a potential corresponding to passive behavior (as shown in Figure 6A), the corrosion rate (current) is much lower than if the cathodic and anodic reactions intersect at a potential corresponding to transpassive behavior (Figure 6B). 17
Galvanic corrosion occurs when dissimilar metals are electrically coupled and exposed to a corrosive environment. Galvanic coupling can cause the corrosion current and corrosion potential to vary significantly from the values of the uncoupled metals. The degree of this shift in corrosion behavior depends on the exchange current densities, the slope of polarization curves, and the corrosion potential of the coupled metals. In general, the metal that has a lower corrosion potential in a given environment will act as the anode in the galvanic reaction, and will be preferentially corroded. Conversely, the metal which has a higher corrosion potential provides a surface on which the cathodic reaction can occur, and will be protected [18, 19, 25]. Galvanic corrosion can occur on a microscopic scale in multi-phase alloys due to differences in the corrosion potentials of their microconstituents. Intergranular corrosion commonly occurs along grain boundaries due to microgalvanic coupling between grain boundary precipitates and precipitate free zone (PFZ) [18, 19, 23, 26]. The PFZ is a solute-depleted layer adjacent to the grain boundary. Propagation of IGC generally requires that the corrosion potential between the grain boundary precipitate and PFZ be greater than 100 mv, and that the grain boundary precipitates contributing to IGC be continuous along the grain boundary [26]. 2.4 Stress Corrosion Cracking Stress corrosion cracking (SCC) is a slow crack growth (typically < 10-6 m/s) phenomenon that occurs when a material is loaded in tension and exposed to a specific corrosive environment. SCC is a primary engineering concern, as it generally results in brittle failure of a nominally ductile material at relatively low applied 18
stresses. SCC failure often occurs at tensile loads well below the yield strength of the bulk material. The tensile stresses may be externally applied or they may be residual stresses from the manufacturing process. Because cracks are often not visible, and there is rarely macroscopic evidence of mechanical deformation of the bulk material, SCC failures often occur without warning. Stress corrosion cracking is broadly associated with materials that demonstrate active-passive corrosion behavior, and SCC failure generally occurs when a material at an electrochemical potential near the transition between active and passive behavior or between passive and transpassive behavior [27]. Growth of SCC cracks is often divided into three distinct regimes: a) Crack initiation and stage I crack growth, b) Steady-state (Stage II) crack growth, and c) Stage III crack growth and Catastrophic failure [19, 27]. Figure 3 schematically depicts the evolution of SCC crack growth with increasing stress intensity. Experimental distinction of the three regimes can be difficult because there is a slow and continuous transition between them. SCC initiation occurs when the stress intensity reaches a critical value, KISCC. The value of KISCC is dependent upon both the material and service environment. SCC initiation sites may be preexisting defects in the material (surface scratch, inclusion, intermetallic phase, etc), or they can be generated by exposure to a corrosive environment during service (breach in passive film, corrosion pits, etc.). Final SCC failure occurs when the crack has grown to a length in which the applied stress intensity exceeds the critical stress intensity, KIC, for the remaining ligament. [18, 19, 28, 29]. 19
Log Crack Growth Rate Crack Growth Rate I II III K ISCC Stress IntensityK IC Stress Intensity Figure 7: Typical relationship between SC crack growth and stress intensity. The three regimes of SCC are indicated. Stress corrosion cracks are fractographically characterized as having sharp, branched crack tips that may be either transgranular or intergranular [19, 25, 30, 31]. There is rarely evidence of corrosion products on the fracture surfaces of SCC failures. The underlying mechanisms for SCC are not yet fully understood. There are two general classes of mechanisms that have been proposed to explain SCC in various material systems [19, 27]. Some researchers argue that SCC is essentially a hydrogen embrittlement phenomenon [19, 27, 32-35]. There are two general models that have been proposed 20
to explain hydrogen embrittlement; hydrogen enhanced decohesion (HED), and hydrogen enhanced localized plasticity (HELP). According to the HED model, atomic hydrogen accumulates at trapping sites such as dislocations or cracks and causes a localized weakening of the lattice [33, 34, 36]. According to the HELP model enhanced plasticity occurs at the crack tip due to absorbed atomic H [32]. Some researchers have attempted to test a hydrogen embrittlement mechanism qualitatively by adding a hydrogen recombination poison (HRP) to the test environment [14, 21, 37]. A hydrogen recombination poison slows the recombination of Hads (Equation 4), thereby increasing the concentration of atomic H in the material. The increased concentration of atomic H in the material tends to magnify the effects hydrogen embrittlement. The As 3+ ion is a commonly used HRP. Small amounts of As 3+ can be added to the environment by dissolving As2O3 into the test solution. The solubility limit of As2O3 in water is ~20 g/l, though only a small concentration (0.3 g/l) is necessary to magnify the effects of hydrogen embrittlement. 21
Figure 8: Schematic of a hydrogen embrittlement of SCC. Atomic hydrogen generated by the cathodic reaction is absorbed, and migrates to the crack tip thus facilitating crack growth by hydrogen embrittlement. Other researchers argue that SCC is a highly localized dissolution phenomenon caused by a discontinuity in the passive film at a crack tip [19, 30, 35] (Figure 9). In dissolution based models of SCC, the passive film at the crack tip ruptures with applied stress, allowing rapid dissolution of the freshly exposed material. The dissolution rate at the crack tip is related to local electrochemical properties of the material and environment. 22
Figure 9: Schematic of an anodic dissolution mechanism of SCC. The passive film becomes unstable at the crack tip, thereby facilitating crack advance due to enhanced dissolution at the crack tip. The local environment within a stress-corrosion crack often behaves as an isolated system, and may be much different from that surrounding environment. For example, when 7075 aluminum alloy is exposed to an aqueous salt water environment, the ph near the crack tip remains relatively constant at ph~3.5 when the applied stress intensity factor is greater than KISCC, regardless of the ph of exterior environment [38-41]. Some researchers have argued that the isolated nature of the crack tip environment lowers the concentration of dissolved O2, thereby reducing the local ph if the bulk solution is near neutral [42]. Others have observed that the ph within a stress-corrosion crack in an Al alloy is controlled by thermodynamic equilibrium between Al 3+ and a solid species within the system (such as Al(OH)3 or Al2O3) [39, 40, 43, 44]. A gradient in electrical potential has also been observed 23
between the electrolyte near the tip of SC cracks and the electrolyte in the bulk environment. [45]. The gradient in potential has been attributed to a difference in chemical potential between the active crack tip and the passive crack flanks with applied stress. The difference in potential between the crack tip and crack flank is thought to lead to enhanced dissolution at the crack tip, or a buildup of atomic H at the crack tip. There do not appear to have been any studies on the local environment within stress corrosion cracks of AA6005A. Although a significant volume of research has been devoted to developing and proving a single explanation for SCC, there has been no universal acceptance of any single mechanism to explain SCC to date [30, 31]. Such an investigation was beyond the scope of the research proposed here, though experiments designed to clarify the mechanism of SCC in AA6005A extrusions were performed. 24
3 Hypotheses and Literature Review There are two primary hypotheses on which this research program was based. These hypotheses are: 1) Metallurgical and environmental conditions that promote IGC susceptibility in the elongated grain structure of AA6005A extrusions, will also promote SCC susceptibility. 2) The mechanism of SCC in AA6005A extrusions is enhanced anodic dissolution at the crack tip due to combined effects of applied load and local electrochemical reactions at the crack tip. 3.1 IGC and SCC Susceptibility of AA6005A: Literature Review In aluminum alloys, SCC is an intergranular phenomenon [27]. Furthermore, conditions (material and environmental) that promote IGC have been shown to promote SCC in a number of different aluminum alloys. Liu et al. observed a continuous increase in IGC penetration rate with increasing tensile stress in underaged AA2024 when exposed to a neutral saltwater environment [13, 46]. In other work, Dymek demonstrated that SCC and IGC resistances in AA2519 alloy are simultaneously improved by cold working and decreasing the copper content to promote a more uniform distribution of precipitates [47]. This direct relationship between IGC and SCC has also been observed in 5xxx and 7xxx alloys [31, 48-51]. These observations suggest that metallurgical and environmental conditions that promote IGC in AA6005A extrusions will also promote SCC, in accordance with 25
hypothesis 1. Though the IGC behavior of 6xxx alloys has been well documented [4-8, 52-54], no study linking IGC and SCC susceptibility in AA6005A exists to date. Nisanciaglu and coworkers conducted a series of studies on the IGC behavior of unstressed AlMgSi(Cu) extrusions with compositions similar to AA6005A and containing between 0.02 and 0.2 wt.% Cu [4-8]. These studies investigated the effects of Cu content and thermal history on the corrosion behavior of the equiaxed grain structure at the extruded surfaces. It was determined that the equiaxed grain structure Cu, is in an underaged condition, and is slow quenched from extrusion temperature. The authors suggest that this increased susceptibility to IGC is due to microgalvanic coupling between the Q-phase precipitates (Al4Mg8Si7Cu2) and the PFZ along grain boundaries. The Q-phase, which has a higher corrosion potential than the aluminum matrix, was found to form a semi-continuous film along the grain boundaries in the equiaxed grain structure when the material was in an underaged condition. Artificial aging coarsened the Cu-rich film to form discrete Q-phase precipitates, which these authors suggest interrupts the cathodic path thus improving IGC resistance of the material. No study on the IGC behavior of the elongated grain structure of at the core of AA6005A extrusions exists to date. Press quenched extrusions of AA6005A contain approximately 95% elongated grain structure by volume (Figure 1). It is therefore necessary to conduct a study on the IGC behavior of the elongated grain structure in order to test the first hypothesis. 26
3.2 Mechanism of SCC in AA6005A: Literature Review Burliegh published a broad review of studies on SCC of wrought aluminum alloys [30]. A dissolution mechanism was generally favored to explain SCC in 2xxx alloys, whereas, whereas a hydrogen embrittlement mechanism was favored for SCC of 7xxx alloys. The second hypothesis that was examined by this research was anodic dissolution aggravated by applied stress is the mechanism of SCC in AA6005A extrusions. Those supporting a dissolution mechanism in 2xxx alloys have observed that grain boundary dissolution will occur with or without applied stress, but that the dissolution is accelerated by applied stress [55] or applied anodic overpotential [56]. Susceptibility to IGC and SCC in 2xxx alloys is generally attributed to microgalvanic coupling between Cu-containing grain boundary precipitates (GBPs) and the Al matrix. The GBPs in this case have a higher corrosion potential than the Al matrix, thereby act as the cathode in the microgalvanic reaction [13, 30, 46, 47, 57, 58]. It is known that AA6005A extrusions with elevated copper content have demonstrated IGC susceptibility due to the presence of GBPs that are cathodic relative to the PFZ [4-8]. It is thus possible that SCC in AA6005A extrusions will be analogous to 2xxx alloys due to these similarities in grain boundary chemistry and corrosion behavior. Though the mechanism of SCC in AA6005A is hypothesized to involve anodic dissolution, it is necessary to also consider the possibility that a hydrogen embrittlement (HE) mechanism may contribute to SCC in AA6005A. Numerous studies have been published which studied the effects of ageing treatment and alloy 27
composition HE susceptibility of 7xxx alloys [59-62]. Knight found that decreased copper content and underaging tended to increase the open circuit corrosion potential near a stress corrosion crack tip in AA7075 and AA7079. These conditions were also found to increase stage II crack velocity. This behavior was attributed to a decrease in copper content within GBPs, thereby rendering the GBPs more anodic relative to the PFZ. In this case, the GBP was found to act as the anode and the PFZ as the cathode in the corrosion reaction. It was argued that this increase in driving force for the corrosion reaction accelerated hydrogen production, thereby increasing the likelihood that atomic hydrogen may be absorbed into the alloy [62]. In general, susceptibility to SCC in 7xxx alloys has been attributed to copper replacing some of the zinc in MgZn2 in GBPs. The presence of the copper tends to increase the corrosion potential of the GBP to a level more similar to that of the PFZ, thereby decreasing the thermodynamic driving force for the electrochemical reactions governing SCC. It is noteworthy that in the case of 7xxx alloys that thought to be susceptible to SCC by a HE mechanism, the grain boundary precipitates are active relative to the PFZ, and act as the anode in the microgalvanic reaction. Conversely, in the case of 2xxx alloys, which are susceptible to SCC by an anodic dissolution mechanism, the grain boundary precipitates are noble relative to the PFZ, and serve as a cathode in the microgalvanic reaction. From an electrochemical standpoint, extrusions of the alloy AA6005A are known to have grain boundary microstructure similar to that of 2xxx alloys. This similarity in electrochemical behavior at the grain boundaries served as the basis for formulated the second hypothesis. 28
There do not appear to have been any studies published on the mechanisms of SCC in AA6005A. Therefore experiments designed to test both anodic dissolution and hydrogen embrittlement phenomena were carried out to determine the fundamental mechanism of SCC in AA6005A. 29
4 Experimental Methods and Results 4.1 Materials Sections of AA6005A extrusion were obtained from a commercial vendor. The nominal composition of the material used in the experiments is given in Table 4. Note that the elevated Cu content is in the range where IGC susceptibility would be expected based on the observations of the Nisanciaglu group [4-8]. The extrusions were received in an as-extruded state (i.e. no post-extrusion thermal treatment). The sample thickness was 3.175 mm for all materials used in this study. The extrusions were air quenched, and the reduction ratio was 44:1. Table 4: Composition of AA6005A extrusions used in experiments. All values are in weight percent. Si Fe Cu Mn Mg Ti Zn Ni Al 0.590 0.195 0.178 0.115 0.434 0.033 0.000 0.005 Balance Samples cut from the extrusions were aged in a laboratory furnace to a T4 (0 hr at 185 C), T6 (6 hr at 185 C), or OA (24 hr at 185 C). The T6 temper tempering procedure was found to give maximum hardness for the material tested. The average yield and tensile stresses for each of the tempers investigated are given in Table 5. Table 5: Yield and tensile stresses for AA6005A extrusions with varied heat treatment. Age Treatment Yield Stress (MPa) Tensile Strength (MPa) T4 155 205 T6 255 300 OA 250 300 30
The coordinate system used to describe the different directions in the material is illustrated in Figure 10. Direction 1 corresponds to the extrusion direction, direction 2 corresponds to the through thickness direction, and direction 3 corresponds to the transverse direction. Figure 10: Definition of coordinate system used to describe specimens. Directions 1, 2, and 3 correspond to the extrusion direction, through thickness direction, and transverse direction, respectively. 4.2 Electrochemical Behavior of AA6005A Extrusions The first step in characterizing the corrosion behavior of the elongated grain structure in AA6005A extrusions was to conduct experiments designed to understand the effects of environment and heat treatment on the bulk electrochemical behavior of the alloy. It is known that the local environment within an occluded region in an IGC or SCC path may differ significantly from that of the external environment. The experiments described in this section were therefore designed to give insight to the electrochemical behavior of within the occluded regions of the alloy as well as understand the bulk electrochemical behavior of the material. The results from these 31
experiments served as a basis for drawing conclusions from IGC and SCC experiments. 4.2.1 Experimental Methods - Polarization Experiments The effects of heat treatment and environment on the electrochemical behavior of AA6005A extrusions were studied by conducting polarization measurements using an EG&G potentiostat/galavnostat. Specimens were aged to a T4, T6 or OA condition prior to preparation. The specimens were machined into 1cm 1cm squares using a CNC end mill. A small ribbon of stainless steel wire was attached to each specimen using conductive silver paste. The stainless steel wire served as an electrical lead to the specimen in the polarization experiments, and did not contact the electrolyte during the experiments. The prepared specimens were mounted in two-part epoxy, and the 1 cm 2 exposed surface was mechanically ground to a 600g finish in 4 steps to fully remove the equiaxed grain structure. The specimen configuration is illustrated in Figure 11. 32
Figure 11: Sample configuration used in polarization experiments for AA6005A extrusions. The experimental setup for the polarization measurements is schematically illustrated in Figure 12. The prepared specimens were placed in the aqueous test solution, and a 3 mm diameter luggin probe was placed near the specimen surface. The luggin probe senses the potential of the solution in the vicinity of the sample, and the potentiostat allows the sample to be held at known values of electrochemical potential during the polarization experiments. A platinum counter electrode with a surface area of 2 cm 2 was placed in the test solution near the sample. A saturated calomel reference electrode (SCE) was immersed in solution of saturated KCl in a separate container. A salt bridge containing saturated KCl solution was used to connect the luggin to the SCE reference electrode. The potential between the specimen and the SCE was scanned from -2.0 V to 0.5 V vs. SCE to yield both 33
cathodic and anodic segments of the polarization curve. The current density of the corrosion reaction (i) was measured between the counter electrode and the specimen, and was plotted against the applied the potential (V vs. SCE). Once the experiment was appropriately assembled, the system was allowed to equilibrate for 180 seconds prior to beginning the polarization measurements. Upon reaching equilibration, the specimens were held at the starting potential (-2 V vs. SCE) for 30 seconds. The potential was then scanned in a stepwise manner. The step size was 1 mv and the dwell time was 0.1 s. Figure 12: Experimental setup for conducting polarization measurements on AA6005A extrusions The polarization experiments were conducted in 3.5% NaCl solutions with 1.20 < ph < 5.50. The ph was adjusted by adding HCl to the solutions. The ph of the solution without HCl addition was approximately 5.5. A small amount (0.3 g/l) of 34
As2O3 was added to the solution for some experiments to study the effects of a hydrogen recombination poison on the polarization behavior of AA6005A-T6 extrusions. 4.2.2 Results and Discussion Polarization Experiments The effect of ph on the anodic polarization behavior of AA6005A-T6 exposed to an aqueous solution of 3.5% NaCl is illustrated in Figure 13. The stability of the passive layer on AA6005A-T6 depended on ph of the test solution, which is consistent with what would be expected from the Pourbaix diagram for Al (Figure 2). The material exhibited passive behavior over a large range of applied potential when the solution was in the range 3.00 ph 5.50. No notable range of passive behavior was exhibited when the solution was at ph 35
Figure 13: Effect of ph on the polarization behavior of AA6005A-T6 in aerated 3.5% NaCl. The values of average corrosion potential and corrosion current density for each solution ph are indicated. The corrosion potential of AA6005A-T6 at each value of solution ph was determined by averaging the observed corrosion potentials for at least 5 polarization experiments (Figure 14). The standard deviation in these measurements was taken as the experimental error. A large decrease (~0.5 V) in corrosion potential was observed when the ph of the solution was increased above 2.0. This large shift in corrosion potential was explained by considering the effects of ph on the stability of the Al2O3 passive film. Kaesche noted that the high resistivity of an Al2O3 passive film tended to slow the rate of the cathodic reaction at the surface of the material [24]. Slowing the 36
rate of the cathodic reaction would tend to shift the exchange current density of the reaction to a lower value, thereby causing the cathodic polarization curve to intersect the anodic polarization curve at a lower value of potential (similar to Figure 6). When ph < 4.0, it is known that the passive film on Al becomes thermodynamically unstable (Figure 2), but dissolves very slowly [18]. Therefore, the observed polarization behavior of the material can represent the polarization behavior of the passive films even when ph < 4.0. The data presented in Figure 14 suggests that under the conditions in these polarization experiments a passive film on AA6005A- T6 dissolves slowly when 3.0 < ph < 5.5, and is fully dissolved when ph < 2.0. Figure 14:Effect of ph on the corrosion potential of AA6005A-T6 exposed to an aqueous solution of 3.5% NaCl. A sharp decrease in corrosion potential was observed when ph > 2.0. 37
The values of corrosion current density, icorr, were extracted from polarization curves using the Tafel analysis procedure described in section 2.3 (Figure 4). Tafel analysis was performed on three polarization curves of AA6005A-T6 for each solution ph. A representative example of Tafel analysis for a sample of AA6005A-T6 exposed to an aerated saltwater solution at ph = 2.0 is illustrated in Figure 15. Notice the very small range of linearity in the anodic portion of the polarization curve. The small range of linearity in the anodic portion of the polarization curve resulted in some error in determining values of icorr. The experimental error in icorr was determined by calculating the standard deviation for at least 5 values of measured current density from each of the experimental conditions. 38
Figure 15: Representative Tafel analysis for AA6005A-T6 exposed to a solution of 3.5% NaCl at ph = 2.0. The relationship between solution ph and icorr is illustrated in Figure 16. The corrosion current density varied with solution ph. Corrosion current densities were found to decrease by approximately 2 orders of magnitude when the ph was increased from 1.2 to 2.0. When the solution ph was greater than 2.0, the corrosion current remained relatively constant at approximately 5.3 10-5 A/cm 2. 39
Figure 16: Effect of solution ph on the corrosion current of AA6005A-T6 exposed to an aqueous solution of 3.5% NaCl. The corrosion current decreased by two orders of magnitude when 1.2 approximately 5.3 10-5 when 2.0 The effect of heat treatment on the polarization behavior of AA6005A extrusions was examined by performing polarization measurements on samples in a T4, T6, or OA temper in solutions of 3.5% NaCl with 1.20 < ph < 5.50. Figure 17 illustrates the effects of heat treatment on the polarization behavior of AA6005A exposed to a solution at ph = 1.50. Heat treatment does not appear have a significant influence on the bulk polarization behavior of the material. A similar relationship was found to be true for solutions with 1.20 < ph <5.50. These results suggest that 40
electrochemical reactions participating in the overall corrosion reaction do not depend significantly on the heat treatment of the material. Figure 17: Effect of heat treatment on the polarization behavior of AA6005A extrusions exposed to 3.5% NaCl at ph = 1.50. The overall polarization does not vary significantly with heat treatment, which indicates that cathodic and anodic reactions involved in the overall corrosion reaction do not depend on heat treatment. The effect of adding a hydrogen recombination poison to an aerated saltwater solution on the polarization behavior of AA6005A-T6 is illustrated by polarization curves in Figure 18. Adding As 3+ to ph =1.50 solution resulted in a slight decrease in ECorr and icorr when the bulk solution ph was 1.50. When the bulk solution ph was 41
3.00, the presence of As 3+ resulted in a larger decrease in ECorr and icorr. Note that there is some noise near ECorr in the polarization curve for the sample tested without As2O3 at ph = 3.00. This noise is random, and does not represent the actual polarization behavior of the material. The presence of a hydrogen recombination poison should not alter the operating anodic reaction; therefore these results suggest that As 3 may alter the cathodic reaction slightly. It is known that dissolved As 3+ tends to slow the recombination of Hads, thereby slowing the kinetics of the cathodic reaction [20, 21, 63]. The results presented in Figure 18B are consistent with this assertion; the lower observed values of icorr and ECorr with the addition of As2O3 to the aerated saltwater solutions suggest a decrease in the exchange current density for the cathodic reaction. These results also suggest that adding As2O3 to the aerated saltwater solutions may be an effective method to test qualitatively for a hydrogen embrittlement mechanism of SCC in AA6005A extrusions. 42
Figure 18: Effect of a hydrogen recombination poison on the polarization behavior of AA6005A-T6. A) The presence of As2O3 does not alter the overall corrosion reaction when ph = 1.50. B) The presence of As2O3 decreases the corrosion potential and corrosion slightly current when ph=3.00. The scale for current density is shared for A and B. 43
4.3 IGC of the Elongated Grain Structure in AA6005A 4.3.1 Experimental Methods IGC of AA6005A The effects of heat treatment and environment on IGC susceptibility of the elongated grain structure in AA6005A extrusions were studied by conducting immersion tests. All immersion tests were carried out in solutions of 3.5% NaCl with 1.20 < ph < 2.00. The ph was adjusted using HCl. Samples were tested in a T4, T6, or OA temper. Rectangular samples measuring 2.54 cm 1.27 cm were machined using a CNC end mill. The extrusion surfaces (1-3 planes) were ground and polished to a 1 m finish to fully remove the equiaxed layer. The machined surfaces (1-2, and 2-3 planes) were polished to a 1 m finish to limit the effects of residual stresses created from the machining process. All samples were degreased in a solution containing 5% NaOH at 50-60 C for 5 min. This degreasing procedure served two primary purposes: 1) To remove any residual organic matter on the surface of the material, and 2) To expose IGC initiation sites (e.g. constituent particles). The degreased samples were rinsed in laboratory ethanol and water and stored in a desiccator prior to immersion testing. The samples were stored for sufficiently long periods of time prior to immersion testing to allow repassivation of the alloy. All samples were handled with gloved hands, and care was taken to avoid any contamination on the sample surfaces subsequent to degreasing. Immersion testing was conducted by suspending the samples in the test solution using monofilament fishing line for a times ranging from 2 to 576 hrs. The 44
modes and depths of corrosion attack along all three directions (Figure 10) were characterized using standard metallographic practices. The structure and morphology of the grain boundary precipitates in the elongated grain structure was characterized using transmission electron microscopy (TEM) and energy dispersive x-ray spectroscopy (EDS). The purpose of the TEM examination was to determine if there is a relationship between grain boundary microstructure and IGC susceptibility. TEM foils were prepared by thinning samples of all age treatments to approximately 100 by abrasive grinding and polishing. Small (3 mm diameter) disks were punched from the thinned samples. Final thinning was conducted using a double-jet electropolisher. The electrolyte was a solution consisting of 25% HNO3 and 75% methanol. The temperature of the electrolyte was held at -25 C during electropolishing. Electropolishing was carried out 30 V. 4.3.2 Results and Discussion IGC of AA6005A The mode of corrosion attack in the elongated grain structure when tested in a solution of 3.5% NaCl at ph = 1.20 was found to depend on heat treatment, as illustrated in Figure 19. When the alloy was in a T4 temper, uniform IGC was observed along directions in the elongated grain structure. When the alloy was in a T6 temper, a IGC was observed along all directions, though there was some evidence of pitting. When the alloy was in an OA temper, local pitting was observed along all directions. The relationship between post-extrusion thermal treatment and mode of corrosion attack in the elongated grain structure observed here is similar to that reported in the equiaxed grain structure [4, 7]. 45
Figure 19: Effect of age treatment on the mode of corrosion attack along the extrusion direction. All samples were tested in 3.5% NaCl at ph=1.20 for 24 hrs. A) Pure IGC was observed when the material was in a T4 temper. B) IGC with some evidence of pitting was observed when the material was in a T6 temper. C) Local pitting was observed when the material was in an OA temper. Transmission electron microscopy revealed that the morphology of the grain boundary precipitates in the elongated grain structure depends on heat treatment. A continuous film containing an excess of Cu was observed in samples in a T4 condition (Figure 20). The Cu-rich film was still present when the material was in a T6 condition, but there was evidence that the film began to coarsen to form grain boundary precipitates adjacent to the film (Figure 21). EDS analysis demonstrated that the grain boundary precipitates contained an excess of Cu, Mg, and Si. The Curich film had completely transformed into discrete grain boundary precipitates containing large amounts of Cu, Mg, and Si when the material was in an OA condition (Figure 22). 46
Figure 20: Core grain boundary microstructure of AA6005A-T4. A continuous film with elevated Cu content was observed along the grain boundaries. 47
Figure 21: Core grain boundary microstructure of AA6005A-T6. Elevated Cu, Mg, and Si contents were observed along the grain boundary. The Cu-rich film was present along the grain boundaries, but was beginning to coarsen to form discrete particles upon aging to a T6 condition. 48
Figure 22: Core grain boundary microstructure of AA6005A-OA. There was no evidence of a continuous film along the grain boundary. The Cu-rich film had coarsened with the overaging heat treatment to form discrete grain boundary precipitates with an excess of Mg and Si. 49
Recall that Nisanciaglu et al. attributed IGC susceptibility in the equiaxed grain structure of AA6005A to the presence of a continuous Cu-rich film along the grain boundaries [4-7].These researchers determined that the Cu-rich film was a Q- phase (Al4Mg8Si7Cu2) precipitate, which was noble relative to the PFZ, thereby resulting in IGC susceptibility by microgalvanic coupling between the grain boundary precipitates and the PFZ. Results presented in Figures 19-22 are consistent with Nisanciaglu s argument. A continuous Cu-rich film was observed along the grain boundaries in the elongated structure when the material was in a T4 and T6 temper, and the elongated structure was susceptible to IGC in these conditions. When the material was in an OA temper, the Cu-rich film was fully transformed into discrete grain boundary precipitates and the primary mode of corrosion attack was pitting. The effects of ph on the severity of corrosion attack along the extrusion direction are illustrated in Figure 23. Increasing the ph of the solution to 1.50 yielded similar depth and severity of corrosion attack in the elongated grain structure as was observed in when the material was tested in a ph = 1.20 saltwater solution. Negligible corrosion attack was observed when the samples were exposed to a saltwater solution at ph = 2.00. The large decrease in severity IGC attack with increasing ph is consistent with the polarization results that indicated a decrease in corrosion when the solution ph was increased to 2.00 from 1.50 (Figure 16). 50
Figure 23: Effect of ph on the severity of IGC in AA6005A-T6 exposed to 3.5% NaCl at A) ph = 1.2, B) ph = 1.5, and C) ph = 2.0 Corrosion testing revealed that the depth of corrosion attack is highly anisotropic in the elongated grain structure when the material was in a T4 or T6 temper (Figure 24). Intergranular attack tended to penetrate most rapidly along direction 1, and least rapidly along direction 2. This anisotropic behavior is graphically illustrated in Figure 25 and Figure 26. Two possible origins for this anisotropic corrosion attack were considered. The first is that the thermomechanical processing (extrusion + heat treatment) might result in strong texturing in the elongated grain structure, thereby yielding in longitudinal grain boundary structures that are more susceptible to IGC due than the grain boundary structures along directions 2 and 3. The second possible reason investigated is that the corrosion anisotropy simply results from elongation of the grains of the extrusion core. The elongated grains provide a less tortuous intergranular path along the extrusion direction than in the transverse or through-thickness directions. Experiments designed to test these two concepts are detailed in the following paragraphs. 51
Figure 24: Typical anisotropic IGC attack observed in the elongated grain structure of AA6005A-T4. A) IGC along direction 1. B) IGC along direction 2. C) IGC along direction 3. Figure 25: Maximum observed depth of IGC attack in the elongated grain structure along directions 1 ( ), 2 ( ), and 3( ) for AA6005A-T4. 52
Figure 26: Maximum observed depth of IGC attack in the elongated grain structure along directions 1 ( ), 2 ( ), and 3( ) for AA6005A-T6. The texture of the elongated grain structure was determined by generating (111), (200), and (220) X-Ray pole figures on a surface normal to direction 2 using Cu radiation. Texture analysis was conducted on samples having both T4 and T6 heat treatments. Electron backscatter diffraction (EBSD) was also conducted on surfaces normal to direction 2 in specimens with both T4 and T6 age treatments. The EBSD analysis was conducted to supplement the X-Ray pole figure results, and to better understand the effects of grain boundary misorientation on the corrosion susceptibility of the specimens. The (200) X-Ray pole figure of the elongated grain structure in AA6005A-T6 is illustrated in Figure 27. Clustering of X-Ray intensity near the center of the pole 53
figure and at angles of = 90, 180, 270 and 360 to the extrusion direction demonstrate that elongated grain structure has strong cubic texturing with the [100] direction being aligned with the extrusion direction. The texture of the elongated grain structure in AA6005A-T4 was found to be nearly identical to that of AA6005A- T6. Similar texture results were found by EBSD analysis. Such strong cubic texturing is typical in extruded Al alloys [64]. These results indicate that directions 1, 2, and 3 are crystallographically equivalent. If grain boundary structure as influenced by texture was the primary factor influencing the anisotropic corrosion attack, the corrosion attack should be similar along all three directions. Grain boundary structure as influenced by crystallographic texturing does not therefore appear to be the primary source of the observed anisotropy of corrosion attack in the elongated grain structure. 54
Figure 27: (200) X-Ray pole figure of elongated grain structure in AA6005A. E.D. indicates the extrusion direction, and T.D. indicates the transverse direction. Clustering of intensities at =0, 90, 180, and 270 indicates that the elongated structure has strong cubic texturing such that directions 1, 2, and 3 are crystallographically equivalent. The simple three-dimensional model shown in Figure 28, similar to that employed by Zhang [15], was developed to explain the observed anisotropic corrosion attack in the elongated grain structure of AA6005A extrusions. In this model, grains are represented as three-dimensional rectangular bricks, with edge lengths corresponding to nominal grain dimension in each direction, stacked upon one another. The nominal grain dimensions for the elongated grain structure in AA6005A-T4 and AA6005A-T6, as measured using a point intersect technique, were 186 +/- 88 µm along direction 1, 47+/-5 µm along direction 2, and 117+/-50 µm along direction 3. The direction of corrosion penetration in Figure 28 is always along the x- 55
direction, and the values of dx, dy and dz will change to represent penetration along direction s 1, 2 and 3. This is necessary because in the simple grain arrangement of Figure 28, only the x-direction approximates the tortuosity associated with corrosion penetration in the real microstructure. Equation 6 relates the length of the corrosion path along direction x (Lx) to the nominal dimensions of the grains. Figure 28: Three-dimensional geometric model used to describe the anisotropic corrosion attack in the elongated grain structure of AA6005A extrusions. The nominal grain dimensions along directions x, y, and z are dx, dy, and dz, respectively. The maximum observed depth of attack along direction x is ax. The shortest corrosion path to achieve a depth of attack equal to ax is indicated by the bold black line. The heavy black line represents the corrosion path length (Lx), as measured by this model, and is given in Equation 6. Equation 6 = (1+ + 2 ) 56
The model was tested by comparing the corrosion path lengths (Lx) deduced from Equation 6 using the measured grain dimensions along each of the three directions and the measured depth of attack, ax. If geometric anisotropy of the elongated structure is the only important factor determining the maximum depth of attack, the calculated corrosion path lengths, Lx, along the three orthogonal directions (1, 2, and 3) should be similar. Table 6 gives the results from testing the geometric model for AA6005A in the T4 and T6 conditions. Table 6: Calculated corrosion path lengths along all directions for samples in a T4 and T6 temper T4 T6 Exposure Time (hr) 2 12 24 Lx (mm) Lx (mm) 1 2 3 1 2 3 0.264 +/- 0.046 0.408 +/- 0.078 0.552 +/- 0.064 0.258 +/- 0.043 0.648 +/- 0.149 0.840 +/- 0.259 0.262 +/- 0.062 0.444 +/- 0.091 0.480 +/- 0.153 0.184 +/- 0.046 0.324 +/- 0.086 0.456 +/- 0.078 0.124 +/- 0.032 0.276 +/- 0.090 0.384 +/- 0.138 0.114 +/- 0.045 0.408 +/- 0.109 0.408 +/- 0.077 The calculated corrosion path lengths for T4 samples agree reasonably well directions 1 and 3 for each of the exposure times. The calculated corrosion path lengths for T4 samples along direction 2 are larger than along directions 1 and 3 for longer exposure times, but still lie within the experimental margin of error. The corrosion path lengths for samples tested in a T6 condition are shorter than those of 57
samples tested in a T4 condition, indicating that the rate of IGC is lower with this heat treatment. The calculated corrosion path lengths for T6 samples are in good agreement along all directions and exposure times. These results suggest that the observed anisotropy of corrosion attack in the elongated grain structure of extruded AA6005A is related to the geometric anisotropy of the elongated grains, and that the maximum depth of corrosion attack is ultimately determined by the tortuosity of the IGC path. Given that the model described above seems to accurately predict the relationship between corrosion path lengths and observed depth of attack, this simple model will be used in subsequent sections to understand the relationship between IGC and SCC susceptibility of AA6005A extrusions. The calculated corrosion path length (Lx) will hereafter be referred to as the structure-corrected corrosion path length. 4.3.3 Effects of Diffusion on IGC Velocity Additional IGC experiments were conducted with exposure times up to 576 hrs to investigate further the observed decay in IGC velocity with exposure time (Figures 25-26). All of these experiments were conducted on samples of AA6005A- T6 exposed to an aerated solution of 3.5% NaCl at ph = 1.50. The maximum depth of corrosion attack was measured along direction 1 using optical microscopy. Multiple micrographs (at least 5 per sample) were evaluated from three samples to determine the maximum depth of attack for each exposure time. Figure 29 illustrates the decay in IGC penetration rate with exposure time for AA6005A-T6 exposed to 3.5% NaCl at ph = 1.5. The instantaneous IGC velocity at a 58
given exposure time was determined by taking the derivative of the logarithmic function that was fit to the depth vs. exposure time data. A plot of the structure corrected corrosion velocity (VIGC) vs. structure corrected corrosion path length (L) is shown in Figure 30. 59
Figure 29: Structure corrected corrosion path length for AA6005A-T6 exposed to an aerated solution of 3.5% NaCl at ph = 1.5. The rate of IGC penetration decays with exposure time. 60
Figure 30: Structure corrected IGC velocity of with increasing corrosion path length observed in AA6005A-T6 exposed to 3.5% NaCl at ph = 1.5. The velocity of IGC decreases by more than 100X with increasing corrosion path length. If we assume that the anodic (Equation 1) and cathodic (Equation 2) reactions involved in the overall corrosion reaction do not vary with corrosion path length, the mechanism of dissolution should not change with increasing corrosion path length. The large decrease in IGC velocity observed at larger corrosion path lengths must therefore be due to some factor that limits the kinetics of dissolution at the tip of an IGC path. The effects of diffusion of specific ionic species involved in the corrosion reaction in the electrolyte were considered in developing a model to explain the observed decay in IGC velocity. 61
It has been established that the local environment within an IGC (or SCC) path may be different than that of the bulk environment [39, 40, 44, 62, 65]. Because the different local environment within a corrosion path may significantly influence the local corrosion behavior of the alloy, experiments were performed to characterize the local ph and [Al 3+ ] within an occluded region of AA6005A-T6, and examine how these factors may affect the velocity of IGC attack. The effect of corrosion path length on the local ph at the crack tip was qualitatively examined using the sample configuration illustrated in Figure 31. A shallow 5.5 mm wide groove was machined into the surface of the sample to accept a piece of litmus paper. A small triangular 0.1 mm deep channel was machined into the bottom of the groove. The channel was designed to simulate the dimensions of an IGC path. Litmus paper was placed into the groove, and glass slides were attached with spring clips to seal the top and bottom surfaces of the sample. The spring clips did not contact the sample; therefore any possible galvanic effects were avoided. The prepared sample was placed in an aerated solution of 3.5% NaCl at ph=1.50. The solution level was maintained at the top of the 0.1 mm deep channel. The change in ph vs. distance from the free surface was approximately determined by observing the change in color of the litmus paper over time. Typical results of this analysis are summarized in Figure 32. 62
Figure 31: Sample configuration used to qualitatively determine the variation in ph with corrosion depth. A piece of litmus paper was placed in a shallow groove, and the sample was exposed to the test environment. The change in color of the litmus paper was used to qualitatively determine the ph gradient along a simulated IGC path. 63
Figure 32: Variation in ph with time. A) At t = 0s the ph is approximately 1.5 throughout the simulated IGC path. B) At t = 600s, only a small region (approximately 1.5mm from the free surface) is at ph = 1.50. The remainder of the simulated IGC path is at ph > 2.50. The ph within about 1.5 mm of the free surface appeared to remain relatively constant at ph The ph appeared to increase to value of 2.5-3.0 within 2.2 mm of the free surface. These results seem to demonstrate that there is a ph gradient within an IGC path in AA6005A-T6. Also note that the color of the litmus paper after the experiment (Figure 32B) is uniform across its width, and is not constrained to the shallow channel milled along the center of 5.5 mm groove. This is due to the solution wicking toward the outer edges of the litmus paper during the experiment. The results presented in Figure 32 are similar to what has been observed in other wrought aluminum alloy systems, in that the ph of the local environment within a corrosion path is independent of the ph of the bulk environment [38, 39]. In contrast to the results presented in Figure 32, however, most studies of the local environment within a corrosion path of wrought aluminum alloys have been 64
conducted with the bulk solution at a near-neutral ph. In these studies, the local ph within a corrosion path was found to be lower (~3.5) than that of the near-neutral bulk solution. The effect of diffusion path length on the local ph was evaluated in a more quantitative manner using the sample configuration illustrated in Figure 33. Small (0.45 mm diameter) holes were drilled through the thickness of a sample of AA6005A-T6 extrusion to simulate an IGC path. The sample was then milled into a wedge, such that the final length of the holes ranged from 1.2 mm to 2.67 mm. A small circle of filter paper was place atop each of the holes, and the bottom of the sample was exposed to a solution of aerated 3.5% NaCl at 1.0 < ph < 5.5. The solution filled each of the holes by capillary forces. The sample was allowed to equilibrate for 30 minutes, and the ph atop each of the simulated IGC paths was measured using a ph microelectrode. Note that these results give the ph at the tip of a simulated IGC path of a given length, and do not give any direct information about the ph along the length of a given corrosion path. The results of these experiments are summarized in Figure 34. 65
Figure 33: Sample configuration used to determine the local ph at varied IGC path lengths. IGC paths were simulated by drilling 0.45mm diameter holes into a wedge-shaped sample of AA6005A-T6. The ph as a function of IGC path length was determined by measuring the ph of solution on a small piece of filter paper placed atop each of the simulated IGC paths with a microelectrode. 66
Figure 34: Effect of corrosion path length and acidity of bulk environment on the ph of the local environment within a simulated corrosion path. The ph within an occluded region increases to a value of approximately 2.50 when the external ph approximately 4.0 when the bulk ph = 2.50. The ph within an occluded region is similar to that of the bulk solution when the external ph = 5.50. When the ph of the bulk solution was 1.0, the ph at the tip of a simulated corrosion path increased approximately linearly to a value of around 2.3 as the simulated corrosion path length approached 2.7 mm. When the ph of the bulk solution was increased to 1.5, the ph at the tip of a simulated corrosion path increased to a maximum value of 2.5 mm. 67
Increasing the ph of the bulk solution to 2.5 caused the ph at the tip of a simulated corrosion path to increase to 4.0 when the corrosion path length exceeded 1.7 mm. The ph at the tip of a simulated corrosion path was similar to that of the bulk environment when the ph of the external environment was at 5.50. The results illustrated in Figure 34 agree reasonably well with the qualitative results presented in Figure 32, and give valuable insight into the decrease in IGC velocity with increasing penetration depth when the material is exposed to a low-ph aqueous environment. The effects of corrosion path length on the local ph at the tip of a simulated corrosion path when the bulk ph was held at 1.5 were considered in developing a model to explain the decay in IGC velocity with increasing depth of corrosion attack. Equation 7 is an linear fit to the data in Figure 34 for a ph = 1.50 solution. This equation gives the relationship between ph at the tip of a corrosion path and corrosion path length, L, when AA6005A-T6 is exposed to an aerated saltwater solution at ph = 1.5. Equation 7 is only valid for L 2.3 mm since the ph becomes essentially constant at 2.5 at L > 2.3 mm. Equation 7 =0.435 + 1.5 ( ) It is not likely that the observed increase in local ph with increasing corrosion path length was due to a lack of availability of H + at the tip of the corrosion path, as there is an abundance of H + in the bulk environment (low ph), and H + diffuses rapidly in saltwater solutions [66, 67]. It is also unlikely that the observed increase in local ph with increasing corrosion path length is due to a decrease in dissolved O2 content near the tip of a corrosion path, as decreased [O2] generally results in a local 68
decrease in solution ph. The relationship between ph and [Al 3+ ] at the tip of an IGC path was therefore examined, and used to develop a model relating Al 3+ diffusion and IGC velocity in AA6005A-T6 extrusions. Several reports have demonstrated that the ph within a corrosion path in certain Al alloys is ultimately controlled by precipitation of specific solid compounds in the corrosion path [39, 40, 43, 44]. The precipitates controlling the equilibrium ph within a corrosion path of an Al alloy could be Al(OH)3 or some form of Al2O3 [43, 44, 68]. According to these reports, when the solubility product [Al 3+ ][OH] 3 reaches the solubility constant for a specific solid compound, K SP, precipitation occurs, and the ph within the corrosion path is stabilized at a value corresponding to the equilibrium value of [OH - ]. The values of K SP for several solid compounds are given in Table 7. Note that all values of K SP in Table 7 are expressed in terms of the product [Al 3+ ][OH] 3. In his discussion of the stability of Al2O3, Pourbaix indicated that aluminum hydroxide gel (Al(OH)3) existing in a corrosion path is often unstable, and eventually crystallizes to form a hydrated phase of Al2O3 [68]. Pourbaix stated the product [Al 3+ ][OH] 3 can be used as a valid approximation to determine the solubility constant for various forms of Al2O3 since Al(OH)3 is a precursor to the formation of Al2O3. 69
Table 7: Solubility products for several solid species that may control the ph within an IGC path in AA6005A-T6 [68] Name Chemical Formula K SP, [Al 3+ ][OH - ] 3 Hydrargillite Al2O3. 3H2O 5.01 10-37 Bayerite Al2O3. 3H2O 3.16 10-36 Böhmite - Al2O3. 3H2O 1.00 10-34 Corundum - Al2O3 3.98 10-34 Aluminum Hydroxide Al(OH)3 5.01 10-33 Assuming the ph at the tip of an IGC path in AA6005A-T6 is controlled by the precipitation of some solid compound when the alloy is exposed to a low-ph saltwater solution, [Al 3+ ] at the tip of the IGC path can be estimated as: Equation 8 [ ] = [ ] Where [OH - ] is related to the ph at the tip of the IGC path (Equation 7), and K SP is the solubility constant for some solid compound in equilibrium with Al 3+ (from Table 7). An expression for [Al 3+ ] at the tip of a corrosion path in terms of corrosion path length can be found using Equation 7 and applying the relationship [OH - ][H + ]=10-14. Equation 9 [ ] = 14 (0.435 + 1.5) With the approximate value of [Al 3+ ] at the tip of an IGC path known, molar flux of Al 3+ from the tip of an IGC path can be estimated by using a one-dimensional application of Fick s first law: Equation 10 = 70
Where JAl3+ is the molar flux of Al 3+ (in mol/(area time), DAl3+ is the diffusion coefficient of Al 3+ in the electrolyte, dcal3+ is the difference between [Al 3+ ] at the tip of the IGC path and [Al 3+ ] in the external environment, and dx is the diffusion path length. Assuming that Al 3+ diffuses exclusively along an IGC path, dx can be estimated as the structure-corrected corrosion path length, L. The molar flux of Al 3+ can be used to calculate an IGC velocity, supposing that IGC penetration is limited by diffusion of Al 3+ away from the tip of an IGC path. First, assume that the IGC path is a straight-walled rectangular tube with cross sectional area A (Figure 35). In order to advance the IGC path a distance dl, the volume of Al that must be dissolved is AdL. Multiplying this volume by the molar volume of Al (MVAl, 0.1 mol/cm 3 ) gives the total number of moles that must be dissolved to advance the IGC path the distance dl. The dissolution rate within the volume AdL would then be: Equation 11 = Where is the dissolution rate (in mol/time), and dt is the increment of time required to dissolve the volume AdL. Multiplying the molar flux of Al 3+ (Equation 10) by the cross sectional area of the IGC path, A, gives the rate at which Al 3+ ions are migrating through a plane a short distance from the tip of the IGC path, Z (Equation 12). The values of Z and must be equal in order to maintain quasi steady-state onedimensional flux (Equation 13). 71
Equation 12 = = Equation 13 = = = Figure 35: Model of IGC path used to determine IGC velocity. The IGC path was assumed to be a straight-walled rectangular tube with cross sectional area A. The IGC velocity was related to the molar flux by considering the conditions necessary to dissolve a volume of the IGC path with a length dl. By rearranging Equation 13, the value of dl/dt (which is equivalent to IGC velocity) can be determined. Notice that the cross sectional area of the IGC path, A, cancels when solving for dl/dt, indicating that IGC velocity is independent of the size and shape of the IGC path that we have assumed in Figure 35. Inserting the 72
expression for dcal3+ (Equation 9), and applying known values of DAl3+ (4.2 10-6 cm 2 /s, [67]) and MVAl (0.1 mol/cm 3 ), gives an expression for IGC velocity with varying corrosion path length (Equation 14). Equation 14 ( ) = 14 (0.435 + 1.5) The diffusion-based model was tested by plotting VIGC vs. L curves (as predicted by Equation 14) using different values of K SP, and comparing the experimental VIGC vs. L data (Figure 36). The different values of K SP used in testing Equation 14 corresponded to the solubility constants for the different solid species that may be controlling the ph within an IGC path of AA6005A-T6 (Table 7). 73
Figure 36: Test of diffusion-based model to predict IGC velocity in AA6005A-T6. The model seems to accurately model the observed decay in IGC velocity with increasing corrosion path length. However, the observed IGC velocity was somewhat lower than the predicted values of IGC velocity. The general shape of the VIGC vs. L curves predicted by Equation 14 closely resembles the experimentally observed decay in VIGC with increasing corrosion path length. The good agreement in trend between the predicted and experimental VIGC behavior suggests that VIGC in AA6005A-T6 exposed to a low-ph saltwater solution is ultimately limited by the ability to transport Al 3+ from the tip of an IGC path into the external environment. This implies that, at least for the range of corrosion path lengths explored here, the mechanisms of electrochemical dissolution within an IGC path (anodic and cathodic reactions) do not change with increasing corrosion path length. 74
Though the diffusion-based model seems to capture the general trend of VIGC decay in AA6005A-T6, the observed VIGC is slower than the predicted VIGC for all values of K SP in Table 7. There are several possible explanations for this observed discrepancy. First, it is possible that there may be some other solid compound that controls the ph within an IGC path in AA6005A-T6 that was not considered in this work. There are several forms of Al2O3 (such as -Al2O3 and -Al2O3) for which the solubility constant is unknown. It is possible that the solubility constant for some solid compound not considered in this work is much lower, thereby making the predicted and observed values of VIGC agree more precisely. The difference between predicted and observed values of VIGC may also be explained by addressing a key assumption used in developing the diffusion-based model. It was assumed that the [Al 3+ ] gradient is linear within the corrosion path with [Al 3+ ] being greatest at the tip of the corrosion path and negligible in the bulk environment. With this assumption, the model predicts that Al 3+ would migrate away from the tip of an IGC path in a unidirectional manner. It is not likely that the [Al 3+ ] gradient is perfectly linear within a corrosion path. Variations from linearity in the [Al 3+ ] gradient within the corrosion may be caused by a number of factors (such as IGC branching, dissolution along the IGC path, etc.) not captured with the model. Therefore it is likely that Al 3+ can migrate toward the tip of the IGC path to some degree. Adjusting the model to account for possible two-way diffusion of Al 3+ would tend to decrease the predicted VIGC, thereby giving better agreement between the predicted and observed VIGC. 75
4.4 Qualitative measurement of SCC susceptibility in AA6005A Extrusions 4.4.1 Experimental Methods - Qualitative SCC of AA6005A The effects of heat treatment and environment on SCC susceptibility of AA6005A extrusions were qualitatively examined by conducting breaking load tests (BLT) [69]. Breaking load tests involve applying a known tensile stress to a sample while exposing the sample to known environment for a prescribed period of time. In BLT, test samples are exposed to a corrosive environment with an applied stress, and control samples are exposed to a corrosive environment without an applied stress. After the samples have been stressed and exposed for the prescribed amount of time, the combined effects of applied stress and exposure are evaluated by measuring the residual strength of the sample after the exposure. The residual strength of a sample in BLT corresponds to the ultimate tensile stress (UTS) after exposure, which is measured by performing a standard monotonic tensile stress. The value of residual strength is then compared to the UTS of a sample that was exposed to the test solution without an applied stress. The residual strength of samples after BLT is reported as a percentage of retained UTS vs. the UTS of samples that were exposed with no applied stress. A high percentage of retained strength corresponds to good SCC resistance, and a low percentage of retained strength corresponds to poor SCC 76
resistance. Breaking load tests have served as a relatively rapid assessment of SCC susceptibility in a number of Al alloys [58, 70, 71]. Tensile loads ranging from 0.7 y to 1.0 y ( y = the yield strength of the alloy) were applied along direction 3 to modified sub-sized tensile bars using calibrated proof rings. The sample geometry is illustrated in Figure 37.The proof rings were designed to be compliant so that the applied load would remain nearly constant over the duration of the experiments, even if the samples elongated slightly. The displacement of the proof rings was periodically measured to monitor the applied load. The experimental setup is illustrated in Figure 38. Figure 37: Modified sub-sized tensile bar geometry used for BLT. 77
Figure 38: Experimental setup for conducting breaking load tests. A static tensile load was applied to the sample using a calibrated proof ring, and the aqueous environment was circulated through environmental chambers using a gravity fed system. For this work, samples having a T4, T6, or OA temper were tested in aerated solutions of 3.5% NaCl with 0.5 < ph < 2.0. Samples were also exposed to solutions containing 0.3% As2O3 to qualitatively examine the effects of a hydrogen recombination poison (HRP) on SCC susceptibility of AA6005A extrusions. The test solutions were circulated through environmental chambers using a gravity-fed system (Figure 39). The primary reservoir contained 15 L of solution. The solution was aerated by bubbling laboratory air through the solution in the primary reservoir. Each of the environmental chambers contained ~ 1 L of solution, and the flow-rate in each of the chambers was held constant at 0.5 L/min. The grip material was AA6005A to 78
prevent galvanic effects between the samples and grips. The exposure time for all samples was 200 hr. Figure 39: Gravity fed system for conducting qualitative SCC analysis of AA6005A extrusions. 4.4.2 Results and Discussion - Qualitative SCC of AA6005A The effects of heat treatment on the residual strength of AA6005A extrusions exposed to a solution of 3.5% NaCl at ph = 1.00 are illustrated in Figure 40. The error bars correspond to the observed standard deviation for each sample condition. A 79
modest decrease in residual strength with increasing exposure load was observed when the samples were in a T6 and OA temper. The combined effects of an applied load and exposure to the corrosive environment had a negligible influence on the residual strength of samples tested in a T4 temper. These results suggest that AA6005A-T6 and AA6005A-OA may be mildly susceptible to SCC when exposed to a low-ph aqueous saltwater environment with large applied tensile loads. The magnitude of the stresses applied to the samples in these experiments was much larger than the maximum design stress for the CSPP solar frames (See section 0). The solutions used in these experiments was also much more aggressive than a typical industrial marine environment. Since there only a minor (~15%) decrease in residual strength was observed in these experiments, it seems that AA6005A extrusions will be suitable for use in CSPP frames in a typical industrial marine environment. 80
Figure 40: Effect of heat treatment on the residual strength of AA6005A extrusions exposed to 3.5% NaCl at ph=1.0. Increasing the applied load during exposure tended to decrease the residual strength in samples tested in a T6 ( ) and OA ( ) temper. Negligible decrease in residual strength was observed when the samples were tested in a T4 ( ) temper. These results suggest AA6005A may be susceptible to SCC when in a T6 and OA temper. Figure 41 compares the combined effects of exposure and applied stress to the effects of exposure alone for AA6005A-T6 samples exposed to acidified saltwater with ph ranging from 0.5 to 2.0. The applied stress for the loaded samples was 100% y (250 MPa). The combined effects of load and exposure did not result in a decrease in residual strength when ph = 0.50, suggesting that bulk dissolution of the material was the dominant factor in determining the loss in strength in this environment. A 81
small, but statistically significant decrease in residual strength between the loaded and unloaded samples was observed when the material was exposed to a solution with ph = 1.00, suggesting that AA6005A-T6 is most susceptible to SCC in these conditions. When the ph was raised to a value of 2.00, an insignificant decrease in residual strength was observed. These results indicate that AA6005A-T6 may be mildly susceptible to SCC in 3.5% NaCl when 1.00 ph < 2.00. Figure 41: Effect of ph on SCC susceptibility in AA6005A-T6. The combined effects of exposure and applied load did not decrease the residual strength when ph = 0.50. The combined effects of load and exposure resulted in a decrease in residual strength when ph = 1.00. A negligible decrease in residual strength was observed when ph = 2.00. These results indicate that AA6005A-T6 may be susceptible to SCC when 1.00 ph < 2.00 82
The presence of an HRP in a solution containing 3.5% NaCl at ph = 1.00 actually improved the residual strength of AA6005A-T6 (Figure 42). These results suggest that As2O3 effectively slows the cathodic reaction to decrease the rate of dissolution. Also, since As2O3 would tend to magnify the effects of hydrogen absorption during exposure, these results suggest that hydrogen embrittlement is likely not the primary operating mechanism of SCC in AA6005A. Experiments designed to quantify the effects of a hydrogen recombination poison on the SCC susceptibility of AA6005A-T6 are summarized in section 4.5.2. Figure 42: Effect of a hydrogen recombination poison on SCC susceptibility of AA6005A-T6. A minimal decrease in residual strength was observed with the presence of As 3+ in the test environment. These results suggest that hydrogen embrittlement is not an operating mechanism of SCC in AA6005A 83
4.5 Quantitative measurement of SCC in AA6005A Extrusions Although the results from a qualitative assessment of SCC in AA6005A using breaking load tests indicated that the material was only mildly susceptible to SCC, additional experiments to quantify the crack growth behavior of AA6005A-T6 extrusions exposed to an aggressive aqueous environment were conducted 4.5.1 Experimental Methods Quantitative SCC of AA6005A Crack growth rate (SCC-CGR) studies were performed on fatigue pre-cracked compact tensile bars of AA6005A-T6. The value of KIC for the sample configuration used in this work was 30.68 +/- 0.78 MPa m, as measured by conducting fracture toughness tests of the samples in an ambient environment. The thickness of the extruded profiles used in this study were 3.125 mm, which was not sufficient to satisfy plane strain conditions up to fracture, so the data presented here is applicable only to materials of similar thickness. Figure 43 illustrates the sample geometry of the compact tensile (CT) specimens. The CT specimens were prepared using wire electrical discharge machining (EDM). The wire diameter was 0.254 mm. Wire EDM allowed the specimens to be produced without introducing residual stresses that could be present with conventional machining techniques. The total crack length, a, prior to fatigue pre-cracking was 14.605 mm. This initial value of crack length corresponds to the distance between the loading points and the end of the wire EDM notch. The width of the notches before fatigue precracking was ~0.254 mm (approximate width of notch formed by wire EDM). A 84
cyclic tensile load with an amplitude of 2225 N and load ratio R = 0.1 was applied to the CT specimens to induce fatigue pre-cracks. The lengths of the fatigue pre-cracks were approximately equal to the thickness of the samples. All samples were loaded along the 3 direction, and crack growth along direction 1 was measured for the SCC-CGR experiments. Most SCC-CGR measurements were conducted in aerated 3.5% NaCl with ph = 1.50. Some experiments were performed in an aerated solution of 3.5% NaCl at ph =2.0. In addition, the possible significance of a hydrogen embrittlement mechanism was examined by adding 0.3% As2O3 to a ph = 1.50 test solution for a few experiments. 85
Figure 43: Sample geometry of CT specimens used for crack growth rate measurements. The COD gauge which was used to precisely measure the crack opening displacement, d, was mounted at the mouth of the CT specimen. The samples were loaded using proof rings instrumented with strain gauges. The strain gauges were mounted on the ID and OD of the proof rings at the 3 o clock and 9 o clock positions. Load (F) vs. strain (, as measured by strain gauges on proof rings) curves were constructed by applying a range of loads and recording the measured strain. The F vs. calibration was performed for each of the proof rings. 86
Instrumenting the proof rings with strain gauges allowed the applied load, F, to be continually monitored throughout the duration of a SCC-CGR experiment using data acquisition equipment. The compact tensile specimens were instrumented with crack opening displacement (COD) gauges to precisely measure the crack opening displacement (d) at the crack mouth. Crack length (a) was determined from the effective specimen modulus, ME. The modulus is defined as: Equation 15 = Where t is the specimen thickness. As the crack length increased, the modulus of the sample decreased. The M vs. a relationship for the CT specimens used in this work was determined by performing modulus measurements on a sample of known thickness with crack lengths ranging from 14.605 mm to 23.85 mm. The results of this calibration are shown in Figure 44. 87
Figure 44: Modulus vs. crack length calibration of the sample configuration used in this work. The values of F and d for the samples were recorded throughout the duration of the SCC-CGR experiments using data acquisition software. These values were used to calculate the modulus of each sample. The values of modulus were correlated to a crack length using the ME vs. a calibration (Figure 44). The crack length and load values were used to calculate stress intensity using a strain energy release rate technique [72]. The details of the strain energy release rate calibration are given in Appendix A. A schematic of the experimental setup used to determine crack growth rates and stress intensities is illustrated in Figure 45 88
Figure 45: Schematic of setup that was used for SCC-CGR experiments. A static load was applied to a compact tensile sample using a proof ring. The load was monitored using strain gauges attached to the ring, and the crack opening displacement was monitored using a COD gauge. The signal was read by a data acquisition board, and complied on a PC. The recorded data was used to determine the change in modulus over time. The modulus is converted to a crack length using the strain energy release rate calibration technique. The setup for conducting SCC-CGR studies was tested by performing a SCC- CGR experiment on a compact tensile specimen of naturally aged AA7475 sheet exposed to 3.5% NaCl. The SCC behavior of wrought AA7475 is well documented, therefore making it a good model material on which to test the validity of the experimental technique described above. Results from a CGR experiment of naturally aged AA7475 are illustrated in Figure 46. The values of KISCC and the stage II crack velocity were observed to be ~17.9 MPa m and ~2 10-4 mm/s, respectively. The observed value of KISCC corresponds reasonably well to findings of Onoro who found that the value of KISCC ranged from ~8 MPa m to ~22 MPa m in an alloy similar 89
to AA7475 exposed to 3.5% NaCl [65]. The observed value of stage II crack velocity is also similar to that observed by Onoro and Bovard who found the stage II crack velocity in similar alloys to range from ~10-4 mm/s to ~10-3 mm/s in alloys similar to AA7475 [73, 74] It was therefore concluded that the experimental setup permitted accurate measurement of SCC behavior in AA6005A extrusions. Figure 46: Results from CGR experiment of AA7475 sheet exposed to aerated 3.5% NaCl. The values of KISCC and stage II crack growth rate agree well with published literature. These results suggest that the experimental setup used for the quantitative measurement of SCC in AA6005A extrusion is valid. 90
Upon completing SCC-CGR experiments the specimens were fractographically characterized using optical microscopy and scanning electron microscopy (SEM). Optical microscopy was conducted to study the morphology of the cracks. Specific features investigated by optical microscopy included the crack branching, and the shape of the crack front after SCC. SEM was conducted to characterize the mode (brittle vs. ductile, intergranular vs. transgranular, etc.) of cracking along the fracture surface. 4.5.2 Results - Quantitative SCC of AA6005A The stress corrosion crack growth rate (CGR) along direction 1 in AA6005A- T6 extrusions was found to be nearly constant at ~3 10-5 mm/s over a wide range of stress intensities when tested in an aerated solution containing 3.5% NaCl at ph = 1.50 (Figure 47). When KI < 8.5 MPa m, the observed crack velocity was approximately 3 10-6 mm/s, and below this stress intensity the crack growth rate became too small to accurately measure. Though it appears that the da/dt vs. K behavior of AA6005A-T6 may correspond to typical SCC behavior (Figure 7) it should be noted that such a large range of Stage II crack growth is not typically observed in aluminum alloys. It is also noteworthy that the observed crack velocity of ~3 10-5 mm/s at 10 MPa m < KI < 28 MPa m is slow relative to many aluminum alloys [30, 31, 51, 55, 61-63, 74]. For comparison, typical stage II crack growth rates in 7xxx alloys exposed to neutral 91
saltwater solutions with cracks growing along the extrusion direction are approximately 10-5 10-3 mm/s. Figure 47: Crack growth rate of AA6005A-T6 extrusions exposed to aerated 3.5% NaCl at ph = 1.50. The crack growth rate was relatively constant at ~3 10-5 mm/s when 10MPa m < KI < 28 MPa m.. Fractography revealed evidence crack tunneling on the fracture surfaces. Figure 48 illustrates a typical fracture surface observed on AA6005A-T6 after SCC- CGR testing. The crack front advances most rapidly near the core of the material and least rapidly along the surface of the material during SCC testing. The significance of this observed crack tunneling is discussed in section 4.5.4. 92
Figure 48: Typical SEM micgrograph of AA6005A-T6 fracture surface after conducting SCC testing in 3.5% NaCl at ph =1.50 for 40 hrs. Evidence of crack tunneling was observed. Fractures surfaces of AA6005A-T6 CT specimens showed evidence of both brittle intergranular fracture and ductile fracture in regions of SCC (Figure 49). The mix of ductile and brittle fracture along the fracture surface suggests that SCC is occurring along small channels in the material, and the remainder of the material between these channels is failing by overload. The mix of brittle and ductile fracture along the fracture surface suggests that SCC growth is discontinuous along the crack front. In this case, SCC would occur only along discrete corrosion paths (regions of intergranular fracture), and regions between the intergranular SCC are fractured in a ductile manner when the fracture criterion is satisfied for the remaining ligament. 93
Further analysis of the local stress state near the crack tips is discussed in section 4.5.4. Figure 49: SEM micrograph of fracture surface within elongated grain structure of AA6005A-T6 CGR sample exposed to a solution of 3.5% NaCl at ph = 1.5. Micrograph was taken near the tip of the stress corrosion crack at the midplane of the sample. Evidence of both brittle intergranular fracture and ductile fracture were observed in regions of SCC. The morphology of the growing cracks in AA6005A-T6 was further examined by conducting optical microscopy along the 2 direction near the mid-plane of the material (Figure 50). A small spacer was placed near the end of the triangular wire 94
EDM notch prior to unloading the CT samples used in this analysis. The purpose of the spacer was to retain the shape of the crack when the crack growth terminated without applying any additional stress that may distort the sample. The prepared samples were etched using Keller s reagent (2 ml HF + 3 ml HCl + 5 ml HNO3 + 198 ml H2O) to reveal the grain structure. The cracks appeared to advance exclusively along grain boundaries when examined using optical microscopy (Figure 50). The opposing fracture surfaces also appear to mate relatively well, indicating that very little bulk corrosion was occurring within the fracture surface. There was some evidence of crack branching near the crack tip. Crack branching is a feature commonly observed in SCC of Al alloys, though it is often much more extensive than observed here [19]. Furthermore, some evidence of crack blunting was observed behind the crack tip. The mix of brittle and ductile fracture observed along the fracture surface (Figure 49) suggests the crack blunting is likely due to discontinuous crack growth that occurs after local plastic deformation near the crack tip. 95
Figure 50: Morphology of advancing crack in AA6005A-T6 exposed to 3.5% NaCl at ph = 1.5. The total stress corrosion crack length in this sample was 4.24 mm. The cracks appeared to advance along the grain boundaries. There was evidence of crack blunting away from the crack tip, and crack branching near the crack tip. Addition of 0.3% As2O3 to the test solution did not have a significant influence on the observed crack growth rate of the alloy (Figure 51). The average crack velocity in CT specimens tested in a solution containing 0.3% As2O3 was ~3.3 10-5 mm/s, whereas the average crack velocity in CT specimens tested in solutions without 0.3% As2O3 was ~ 3.0 10-5 mm/s. These results are not consistent with what would be expected if SCC in AA6005A-T6 extrusions were primarily a hydrogen 96
embrittlement phenomenon, as there was no enhancement in CGR with the addition of an HRP to the test solution. Figure 51: Effect of a hydrogen recombination poison (As2O3) on the crack growth rate of AA6005A-T6. The addition of As2O3 did not enhance the observed crack growth rate, suggesting that hydrogen embrittlement is not an operating mechanism of SCC in AA6005A-T6. Fractography of SCC-CGR specimens exposed to solutions containing As2O3 revealed mechanisms of crack growth that are similar to those of specimens exposed to solutions without As2O3. A mix of brittle and ductile fracture was observed along the fracture surface in samples tested in the solutions containing As2O3 (Figure 52). These results indicate that the addition of a hydrogen recombination poison to solution does not significantly alter the mechanisms of crack growth in AA6005A-T6, 97
and that the mechanism of SCC in AA6005A-T6 exposed to acidified saltwater is not influenced by changes in the hydrogen discharge reaction. This, in turn, suggests that the SCC mechanism in this alloy could operate primarily by anodic dissolution. 98
Figure 52: Fracture surface of AA6005A-T6 CGR specimen exposed to a solution of 3.5% NaCl + 0.3% As2O3 at ph = 1.5. Micrograph was taken near the tip of the stress corrosion crack at the midplane of the sample. Evidence of brittle and ductile fracture along the fracture surface indicates that the mechanism of crack growth is similar to that of a sample exposed to a solution without As2O3. 4.5.3 Discussion of Quantitative SCC Analysis Recall that diffusion of Al 3+ away from the tip of an IGC path was found to be the primary factor limiting the velocity of IGC in the case of unstressed samples (Section 4.3.3). The possibility that the velocity of SCC in AA6005A-T6 is also 99
limited by diffusion of Al 3+ away from the crack tip was examined by applying the diffusion-based model discussed in section 4.3.3. Figure 53 illustrates the experimentally observed relationship between the structure corrected corrosion velocity and the structure corrected corrosion path length for both loaded CT samples (SCC-CGR) and unstressed (IGC) samples. The structure corrected corrosion velocity (vertical axis) and corrosion path length (horizontal axis) were deduced using Equation 6. The structure-corrected corrosion path length in the dataset for the loaded CT samples ( ) corresponds to the corrosion path length only in regions of SCC (does not include fatigue precrack). The structure corrected corrosion path length in the dataset for unstressed samples ( ) corresponds to the total calculated path length between the external environment and the tip of an IGC path along direction 1. Figure 53 demonstrates that there is minimal difference in corrosion velocity between the stressed and unstressed samples at small corrosion path lengths (< 0.25 mm). As the corrosion path length increases beyond about 0.25 mm, the structure corrected IGC crack velocity for the unstressed samples decreases, while the SCC crack velocity for the loaded CT samples remains approximately constant at ~3 10-5 mm/s. Since the observed SCC velocity was independent of crack length (Figure 53), the effective diffusion path length for Al 3+ away from the crack tip must be constant if diffusion of Al 3+ is a limiting factor to crack growth in loaded CT samples of AA6005A-T6 according to Equation 14. It is unreasonable to assume that the shortest diffusion path length for Al 3+ would be along the direction 1, as the lengths of all 100
cracks (including SCC and fatigue precrack) in the SCC-CGR experiments were larger than the specimen thickness. The length of the cracks along direction 1 are also continuously increasing during SCC-CGR experiments, thereby decreasing the driving force for Al 3+ diffusion along 1 as the cracks become longer (which is inconsistent with observed v vs. L behavior, Figure 53). Therefore if diffusion of Al 3+ away from the crack tip were the limiting factor in determining the velocity of SCC in the case of loaded CT samples, it can be assumed that Al 3+ must migrate along the 2 direction. Figure 53: Structure-corrected corrosion velocity with increasing corrosion depth along direction 1 for stressed ( ) and unstressed ( ) samples. A significant decrease in velocity was observed with increasing corrosion depth in the absence of an applied stress. 101
The effective corrosion (and diffusion) path length, L, along the 2 direction would be approximately equal to the distance between a point on the crack front and the external environment (Figure 54). The crack front was assumed to be a straight line oriented perpendicular to the crack growth direction. This crack front geometry used does not accurately model the crack tunneling observed in the SCC-CGR samples, but should allow reasonable estimation of the diffusion path length for Al 3+ along direction 2. In this case, SCC velocity should not depend on crack length since the effective diffusion path length would not vary with crack length. 102
Figure 54: Effective corrosion (and diffusion) path lengths along direction 2 for stressed SCC-CGR specimens with crack lengths greater than the 1/2 thickness of the sample. When the crack length exceeds the ½ thickness of the sample, the shortest corrosion path length between the crack front and the external environment would correspond to the distance between that point and the external environment along the 2 direction. The effective corrosion path length for point A in this figure is LA. Similarly, the corrosion path lengths for points B and C are LB and LC, respectively.. Equation 14 was applied to calculate the crack front velocity at the centerline of a CT sample, and to generate a profile of SCC velocity along the crack front. These calculations were made assuming Al 3+ diffuses exclusively along direction 2, and the observed ph vs. diffusion path length behavior (Figure 34) is valid for both unstressed and stressed samples. With these assumptions, the velocity at the centerline of a CT specimen was calculated to 3.89 10-7 mm/s, which is ~100X 103
smaller than the observed constant SCC velocity (~3 10-5 mm/s). This result suggests that diffusion of Al 3+ away from the crack tip is not the primary limiting factor in determining the velocity of SCC in AA6005A-T6. Furthermore, if diffusion of Al 3+ away from the crack tips along direction 2 were the limiting factor in determining SCC velocity of AA6005A-T6, the crack velocity would be least along the centerline of the material and greatest along the edges of the material, as shown in Figure 55. The predicted velocity profile at the crack front is not consistent with the observed crack tunneling during SCC-CGR experiments (Figure 48). Therefore, in contrast to IGC in unstressed samples of AA6005A-T6, it does not appear that the SC crack velocity in the case of loaded CT samples is limited by diffusion of Al 3+ along the 2 direction. 104
Figure 55: Calculated velocity profile along the crack front of a CT sample of AA6005A-T6 exposed to 3.5% NaCl at ph = 1.5. The velocities at various points along the crack front were calculated by applying Equation 14. Recall that the addition of a hydrogen recombination poison to the test solution did not have a significant influence the SCC susceptibility of AA6005A-T6. This result suggests that hydrogen embrittlement is not the dominant mechanism of SCC in AA6005A-T6. Additional analysis of the local stress state and electrochemical reactions at an SC crack tip was performed to further investigate the possibility that anodic dissolution may be the primary mechanism of SCC in AA6005A-T6. 105
4.5.4 Effects of Stress Triaxiality and Local Electrochemical Reactions on Stress Corrosion Cracking of AA6005A-T6 Crack tunneling was observed along the fractures surfaces of loaded samples exposed to 3.5% NaCl at ph = 1.5 (Figure 48). In linear elastic fracture mechanics (LEFM), the phenomenon of crack tunneling is generally attributed to a local in maximum stress triaxiality just ahead of the crack tip near the center plane of the material. Factors leading to triaxiality of the stress state at the specimen mid-plane near the crack tip are illustrated schematically in Figure 56. Because normal tractions are absent on the 1-3 surface, that surface is always in a state of plane stress ( 2 = 0). When the plastic zone near the crack tip is large (Figure 56B), through-thickness thinning of the specimen minimizes 2 at the specimen mid-plane thereby minimizing triaxiality of the stress state. When the plastic zone is small (Figure 56A), throughthickness elastic constraint around the crack tip leads to values of 2 that approach the value of 3. Similar reasoning leads to the conclusion that elastic constraint gives values of 1 that are approximately equal to 3. When 1= 2 = 3, a state of perfect stress triaxiality is achieved [72, 75]. The significance of perfect triaxiality is that while the principle stresses ( 1, 2, and 3) may be significant, the shear stresses will vanish. Low shear stresses minimize plastic deformation, and the tensile stresses promote brittle facture over plastic deformation of the material. 106
Figure 56: Effect of plastic zone size on the stress state experienced in a material. Figures A and B are looking at a plane ahead of the crack front along direction 1, as indicated by the dark arrow in the perspective view at the top. A) Surface deformation is limited by a large constraining stress oriented perpendicular to the loading axis when the plastic zone is small. B) Lateral deformation is observed if the plastic zone is sufficiently large. 107
Figure 57 shows the morphology of a crack growing along the direction 1 in a compact tensile sample of AA6005A-T6 after SCC-CGR testing in a solution of 3.5% NaCl at ph = 1.5. The specimen illustrated in Figures 57A-D was prepared by making serial sections of 3-2 planes at different depths along direction 1. Figure 57A shows the morphology of a growing SC crack in the 3-2 plane 1 mm beyond the end of the fatigue precrack. Similarly, Figures 57B-D show the morphology of a growing SC cracking the 3-2 plane 2, 3, and 4 mm beyond the end of the fatigue precrack. The total length of the SC crack for the sample shown in Figure 54 was approximately 4.08 mm, so Figure 57D represents the morphology of the SC crack at a plane near the crack tip. Note that there is negligible plastic deformation along direction 2 at the surface of the specimen at all crack lengths. The lack of deformation along the free surfaces of the sample suggests that there is a region within the sample thickness that does not experience significant shear stresses, and would therefore be experiencing a significant degree of stress triaxiality. 108
Figure 57: Crack morphology at various depths in a compact tensile bar of AA6005A-T6 exposed to 3.5% NaCl at ph = 1.5. The crack is growing along direction 1. A) 1mm beyond fatigue precrack. B) 2mm beyond fatigue precrack. C) 3mm beyond fatigue precrack. D) 4mm beyond fatigue precrack. No evidence of deformation along the 2 direction was observed at any point beyond the fatigue Precrack. Assume the crack tip plastic zone is sufficiently small to satisfy plane strain conditions near the center of the material, the maximum stresses experienced near the crack tip of AA6005A-T6 SCC-CGR specimens can be estimated using the plastic constraint factor (PCF). The PCF is defined as [75]: 109
Equation 16 = Where max is the maximum tensile stress near a crack tip, and y is the bulk yield stress of the material. In the case of plane strain loading, the value of PCF approaches a value of 3 along the plane of the advancing crack [75]. Details of the calculations used to determine the PCF are given in Appendix B. The bulk yield stress of AA6005A-T6 is approximately 250 MPa, thus the maximum stress near the crack tip would be approximately 750 MPa. This probably overestimates the value of maximum stress at the crack tip, as the applied loads for the SCC-CGR experiments in this work correspond to a crack tip stress which is much lower than the bulk yield stress of the alloy according to the relationship KI = (a) 1/2. However, this value gives a reasonable approximation of the stress state near the crack tip. The effect of stress on the chemical potential near a crack tip can be estimated using the Nabarro-Herring (NH) model [76, 77]. The NH model is used to determine the change in free energy associated with a vacancy migrating from an unstressed (crack flank) to a stressed (crack tip) region (Figure 58). Though originally formulated to describe the driving force for high-temperature diffusional creep, the NH model has been applied to understand the driving force for dissolution in the case of SCC [78-82]. The NH model states: Equation 17 = 110
Where is the change in chemical potential associated with vacancy migration to a crack tip, MVAl is the molar volume of Al, and app is the local stress. If we assume the applied stress near the midplane of the CT specimens approaches 750 MPa, and take the molar volume of Al as 0.1 mol/ cm 3, is found to be 7,500 J/mol. Figure 58: Schematic representation of the Nabarro-Herring model. Vacancies migrating from an unstressed region to a region of maximum stress results dissolution of the parent material and a decrease in chemical potential near the crack tip. The change in electrochemical potential at the crack tip due to an applied load was related to the change in chemical potential using Faraday s law [83]: 111
Equation 18 = Where is the change in electrochemical potential, n corresponds to the number of electrons involved in the dissolution reaction (3 for Al), and F is Faraday s constant (96,500 C/mol). Applying equations 17-18, the total change in electrochemical potential at the crack tip due to an applied load was estimated to be approximately -0.026 V. This change in electrochemical potential would shift the half-cell corrosion potential of the anodic reaction (Al = Al 3+ + 3e - ) to a lower value, and should have no effect on the half-cell corrosion potential of the cathodic reaction. Recall from section 4.3.3 that the ph at the tip of a corrosion path varied with corrosion path length. When the ph of the bulk solution was held at 1.5, the ph at the tip of a corrosion path was found to reach an equilibrium value of ~2.5 as the corrosion path length approached 2.3 mm. Assuming the effective corrosion path length is 1.58 mm (1/2 thickness of CT sample) for loaded CT samples of AA6005A- T6, the ph at the tip of the corrosion path is approximately 2.0 when the ph of the bulk solution is 1.5 (Figure 34). In the case of loaded CT samples of A6005A-T6 exposed to 3.5% NaCl at ph = 1.5, the surface area of stressed material exposed to a solution with ph =2.0 would be very small relative to the surface area of material exposed to solution with ph =1.50 (Figure 59). Since electrons can move freely between the crack tip (where they are created by the anodic reaction) to the external surfaces of the sample (where they are consumed by the cathodic reaction), it is reasonable to assume that the anodic and 112
cathodic reactions governing crack growth are occurring at different locations on the CT samples. With this assumption, the cathodic reaction on the unstressed surfaces would follow the polarization curve for AA6005A-T6 exposed to a solution with ph = 1.50, and the anodic reaction at the crack tip would follow the polarization curve for stressed AA6005A-T6 exposed to a solution with ph = 2.0. It is also reasonable to assume that the overall corrosion reaction would be occurring at a potential near the corrosion potential for a sample exposed to a solution with bulk ph = 1.5 since the majority of the sample is unstressed and exposed to the ph = 1.5 solution. 113
Figure 59: Only a small fraction of a loaded compact tensile bar will be exposed to solution at ph = 2.0 when the ph of the bulk solution is held at 1.50. First consider the electrochemical reactions occurring at a stress corrosion crack tip in a loaded CT sample of AA6005A-T6 that is exposed to a solution of 3.5% NaCl at ph =1.5 (Figure 60). In this case, the highly stressed crack tip will be exposed to a solution with ph =2.0, while the majority of the sample (which is in an unstressed state) will be exposed to a solution with ph =1.5. The anodic reaction occurring in the crack tip solution would be shifted downward by ~0.026 V vs. SCE 114
due to the local stress state at the crack tip, and the cathodic reaction would follow the polarization curve for an unloaded sample exposed to a ph =1.5 solution. Since most of the sample is exposed to a ph =1.5 solution, it is reasonable to assume that the anodic reaction at the crack tip will be occurring at the value of ECorr when a sample exposed to the ph =1.5 solution (-0.71 V vs. SCE). With these assumptions, the anodic corrosion current density at the crack tip in the case of a loaded CT sample exposed to a solution of 3.5% NaCl at ph =1.5, i1.5, should be approximately 4.6 10-4 A/cm 2. Figure 60: Predicted polarization behavior at a stress corrosion crack tip for AA6005A-T6 exposed to 3.5% NaCl at ph = 1.50. 115
Now consider the electrochemical reactions occurring at a stress corrosion crack tip in a loaded CT sample of AA6005A-T6 that is exposed to a solution of 3.5% NaCl at ph =2.0 (Figure 61). In this case, the cathodic reaction at the free surface should be occurring at approximately ph = 2.0, and the anodic reaction at the crack tip should be occurring at approximately ph = 3.0, according to the observed L vs. ph relationship (Figure 34). The anodic reaction occurring in the crack tip solution would be shifted downward by ~0.026 V vs. SCE due to the local stress state at the crack tip, and the cathodic reaction would follow the polarization curve for an unstressed sample exposed to a ph =2.0 solution. Since the majority of the sample is in an unstressed state, the anodic reaction at the crack tip should be occurring at a potential approximately equal to the value of ECorr for the bulk sample (-0.792 V vs. SCE). In this case, the corrosion current density at the crack tip, i2.0, would be approximately 3.9 10-5 A/cm 2. This predicted value of corrosion current density for a loaded CT sample of AA6005A-T6 exposed to a ph =2.0 solution is 11.8X lower than the predicted corrosion current density for a sample exposed to a ph = 1.5 solution. Results from these analyses are summarized in Table 8. 116
Figure 61: Predicted polarization behavior at a stress corrosion crack tip for AA6005A-T6 exposed to 3.5% NaCl at ph = 2.0. Table 8: Summary of electrochemical analysis for CT specimens exposed to ph =1.5, and ph =2.0 aerated saltwater solutions with and without an externally applied load. Exposure Conditions Current Density at Crack Tip, i Change in Current Density at Crack tip ph = 2.0, Applied Load 3.9 10-5 A/cm 2 - ph = 1.5, Applied Load 4.6 10-4 A/cm 2 + 11.8X Additional SCC-CGR experiments were conducted on CT samples of AA6005A-T6 exposed to 3.5% NaCl at ph = 2.0 to examine the combined effects of an applied stress and a ph gradient between the crack tip and the bulk solution on the SC crack velocity of the alloy. All experimental methods were identical to those described in section 4.5.1. Since corrosion current density is a direct measure of 117
dissolution rate, the crack observed velocity in should decrease by approximately 11.8X when the ph of the bulk solution is increased from 1.5 to 2.0 if stress-enhanced anodic dissolution is the primary mechanism of SCC in AA6005A-T6. Figure 62 illustrates observed SC crack velocity at varied crack lengths for samples of AA6005A-T6 tested in solutions of 3.5% NaCl at ph=1.5 ( and ph=2.0 (. The shaded grey region in Figure 62 represents the range of observed crack velocities for samples tested in a ph = 2.0 solution. Similar to samples tested in a ph = 1.5 solution, the crack velocity for samples tested in a ph = 2.0 solution did not appear to depend on crack length or applied stress intensity. However, the nominal crack velocity of samples tested in solutions at ph = 2.0 was approximately 10.5X smaller than that of samples tested at ph = 1.5. This observed decrease in SCC velocity at the higher solution ph is consistent with the predicted decrease in SCC velocity per the analyses discussed above. Therefore it appears that SCC velocity in AA6005A-T6 exposed to low-ph saltwater solutions is ultimately controlled by stress-enhanced dissolution at the crack tip. 118
Figure 62: Structure corrected corrosion velocity for loaded CT samples of AA6005A-T6 exposed to 3.5% NaCl at ph=1.5 or ph=2.0. The observed 10.5X decrease in corrosion velocity associated with increasing the ph of the electrolyte from 1.5 to 2.0 is consistent with the predicted decrease in crack tip current density. 119