Matthews Paint. Troubleshooting Guide

Similar documents
Acrylic Enamel Topcoat

Tractor Painting Tips

DuPont Cromax Pro PAINTER S GUIDE

Epoxy Floor Coating Problem Solving Guide

DuPont ChromaOne Acrylic Urethane Single Stage

SC2000 CEMENT BONDING PROCEDURES

3.8 HSP (High Solids Polyurethane)

TECHNICAL DATA RS European Clear EZ N. Webster Street Dayton, OH Phone Toll Free Fax

Product Information. D8115 Matte and D8117 Semi-Gloss Clearcoat System

Summit Racing Equipment s Paint and Auto Refinishing System was developed specifically for the home enthusiast and small shop owner wanting a

BLADE REPAIR INSTRUCTION BOOKLET

You have just purchased the most portable and economical spray chrome system in the world!

Technical Data Sheet L Top coats. Mat Clear

INDUSTRIAL FLOORING INSTALLATION CHALLENGES. James C. Ziegler, ArmorSeal Product Manager Sherwin Williams Cincinnati, Ohio, USA

MARTIN TESTING LABORATORIES (MTL) PAINTS AND COATINGS TESTING CAPABILITIES

GRIP-GARD BC BASECOAT CHROME

VC 104+ Rigid Grade / Rigid Grade Imagine VC 104 Rigid Grade Commercial Customised

Application of Exterior Wood Finishes

Adhesive Recommendation for Altro Flooring. Porous (absorbent) subfloors (most wood subfloors and some concrete)

SCHWARTZ WATER-BASE WOOD FLOOR SEALER AND WATER-BASE PREMIIUM WOOD FLOOR FINISH

PLAS-STICK 2330S PLASTIC ADHESION PROMOTER

CHROME FX PUMP SYSTEM APPLICATION GUIDE

PRISM Low VOC Single Stage Color Flat (76), Satin (77), Semi-Gloss (78), & Gloss (79)

SECTION POLISHED CONCRETE FINISHING

RAPTOR TRUCK BED LINER - BLACK

Chrome Finishing For 3d Powder Prints

basic assumptions refinishing

TROUBLESHOOTING GUIDE FLEXOGRAPHIC INKS

SECTION 623 CONCRETE BONDING COMPOUND, EPOXY MORTAR AND EPOXY POLYMER CONCRETE OVERLAY SECTION CONCRETE BONDING COMPOUND.

STERI-SOFT HIGH FOOT TRAFFIC, ULTRAVIOLET RESISTANT, URETHANE RESILIENT FLOORING SYSTEM, 1/8 GREEN BUILDING FEATURES TYPICAL APPLICATIONS

PLAS-STICK 2322S GENERAL MIXING. DESCRIPTION An adhesion COMPONENTS. MIX RATIO Ready to Spray. POT LIFE Indefinite. ADDITIVES Accelerator:

How to Install Hardwood Flooring Over a Sub Floor

Product Information/Specifications

Intercoastal Paint Company

Scotch-Weld TM. Epoxy Adhesive 1838 B/A Green 1838 B/A Tan 1838-L B/A Translucent. Technical Data February, Product Description

Application Instructions for Avery Dennison Films SF S LTR EZ RS, Conform Chrome

REFLECTIT. Reflectit Application Instructions Spray and Roller DS % Acrylic Coating Providing a Pearlescent Appearance

Minor Cracks in Horizontal Surfaces

BLACK JACK ALL WEATHER ROOF COATING

Training Course Catalog

Surface Information and Preparation Data Sheet (SIPDS) SIPDS No. 1 Interior Wallboards - walls and ceilings

K2 STONE NATURAL VENEER

Solvent Cementing Instructions For Plastic Pipe & Fittings

3 Scotch-Weld TM. Urethane Adhesives 3532 B/A 3535 B/A 3549 B/A. Technical Data March, 2002

REPAIR MANUAL MATERIALS

Eclipse. Technical Data Sheet. Polyurethane topcoat. Product Group

Colorado State University. Durrell Center Roof Repair

Selection, Use, and Care of Brushes

BENTLEY ELEMENTS COLLECTION LVT

Flocking of textiles. Flocked shirt 13. flocking drying cleaning. adhesive. application. creation

RECOATING AND RENEWING SPF ROOFING SYSTEMS

Property Test/Standard Description. semi gloss (35-70) Flash point ISO 3679 Method 1 34 C IED (2010/75/EU) (calculated)

General Surface Preparation

3 Scotch-Weld TM. Structural Adhesive Films AF 6 AF 10 AF 13. Technical Data July, 2001

Scotch-Weld TM. DP410 Off-White. Product Data Sheet. Product Description. Key Features Rapid cure at room temperature; cure rate may be accelerated

SCENIC VIEW SV 10 SECTION SOLAR CONTROL FILMS

Material Product Data Sheet Sealers for Thermal Spray Coatings

Aspect Metal Peel & Stick Tile Installation Guide

High Solids Epoxy System G Intermediate Coating.

Scotch-Weld TM. Acrylic Adhesives. DP8405NS Green. Product Data Sheet. Date: March 2014 Supersedes: August 2013

Technical Data Sheet February 2014

AIRLESS SPRAY SYSTEMS

INDUSTRY RECOMMENDATIONS for Sanding, Sealing Court Lining, Finishing & Resurfacing of Maple Gym Floors

10P20-44 High Solids Epoxy Primer

Contents. Introduction...3. Determine the Type of Floor Finishing Project...4. Things to Think About Before You Start...5. Assemble Materials...

SIGMACOVER 280. PRODUCT DATA SHEET December 10, 2014 (Revision of March 1, 2014) DESCRIPTION

2K P422- Basecoat System. P Solid colour basecoat converter P Basecoat flip controller P High aluminium flip controller

Wecryl Waterproofing System under surfacing supplied by others

PHOENIX Product Data Sheet (Updated on 14-Jan-2012)

TECHNICAL DATA SHEET HAMMERITE METAL PAINT. Smooth Hammered Satin Aerosol

Recommended Procedure For How to Prepare and Paint Carbon Fiber and Composite Parts

ARDEX GUIDE SPECIFICATION ARDEX Exterior Concrete Repair & Resurfacing Polymer-Modified, Cement-Based, Patch & Horizontal Overlay Materials

Additional Information. Paint Application

3 Scotch-Weld TM. Urethane Adhesives 3532 B/A 3535 B/A 3549 B/A. Technical Data January, 2010

RESTORE 10X Advanced Resurfacer FAQs Page 1 of 11

SKIMSTONE APPLICATION INSTRUCTIONS FOR CONCRETE FLOORS

BUILT-UP ROOF COATING SMOOTH and GRANULE SURFACE SPECIFICATION

INSTALLATION INSTRUCTIONS

A complete guide of epoxy coatings for industrial and marine applications. Epoxy Coatings Guide

TrūShine Gel Enamel FAQs

Hardwood Maintenance. WORKBOOK and TIPS of the TRADE

GigaCrete Specification PlasterMax

SIGMAFAST 210. PRODUCT DATA SHEET December 12, 2014 (Revision of April 1, 2013) DESCRIPTION

Construction. 3-part thixotropic epoxy patching mortar. Product Description. Tests

the runnerless types of molds are explained post molding operations are described the basic methods of applied decoration methods are examined

SIGMACOVER 300. PRODUCT DATA SHEET December 12, 2014 (Revision of November 1, 2013) DESCRIPTION

FLOOR TREATMENT 09610

Division 9. SignaFlor Pad and Pour Flooring System

Vinyl Composition Tile Installation System

Packaging Gravure Troubleshooting Guide

Pulley was done with the rust technique shown later

Flexography Troubleshooting Guide

Installation System. Existing Resilient Sheet Floors

DIRECT PRINTING NYLON JACKETS. The Basics

Document Library TS Data Sheet

Mold Preventing I nterior System

Laminating Films - Heat Activated

Property Test/Standard Description. gloss (70-85) Flash point ISO 3679 Method F (100 C) calculated VOC-US/Hong Kong. US EPA method 24 (tested)

Digital Printing: Knowing and Avoiding Imaging and Application Pitfalls with Digital Graphics. Piezo Ink Jet Printing

WATERPROOFING OF WET ROOMS

Transcription:

Matthews Paint Troubleshooting Guide This guide provides frequently asked questions with answers and a list of common problems, what causes the problem, and a general list of corrective actions. Frequently Asked Questions.......................................... 2-4 Troubleshooting Guide Orange Peel..................................................... 4 Dry Spray....................................................... 5 Color Match..................................................... 5 Sags or Runs.................................................... 5 Fisheyes....................................................... 6 Dirt.......................................................... 6 Peeling........................................................ 6 Soft Paint...................................................... 7 Die Back....................................................... 7 Solvent Trap (Popping).............................................. 7 Mottling....................................................... 8 Sand Scratches & Bullseye........................................... 8 Overspray...................................................... 8 760 Pittsburgh Drive Delaware, OH 43015 1.800.323.6593 Fax: 1.800.947.0377 Visit our website at: www.matthewspaint.com Matthews Paint is a trademark of PPG Ohio, Inc. MPC 325 12/10

FAQs Frequently Asked Questions What is the coldest temp I can spray Matthews paint at? Inside and outside: 60-65 degrees minimum. Substrate and paint should also be at these minimum temperatures. What will happen if I do spray below 55 degrees? Product won t crosslink. Do I need a respirator? Yes Yes Yes Supplied Air is recommended for everything. Can Matthews paint be sprayed in a mall while people are present? Not recommended to spray due to vapors. Can you screen print with MAP? Not recommended. MAP isn t designed to be screen applied. What Matthews primers can I put on top of Matthews paint? Epoxy primers U-Prime No wash primers or Polyester Primer Can you put MAP over screen print coatings? Most silk screen materials are enamels, and Matthews may lift enamels. Epoxy and urethane screen prints can be topcoated or cleared with Matthews. Can you put MAP over sign foam? SignFoam Yes, with Polyester Primer, U-Prime or Epoxy. Styrofoam No, it will dissolve foam. Can you apply Matthews over existing coatings? In many cases you can, but each instance should be tested first. What primer is recommended for wood? Results may vary since there are many kinds of wood and wood products. Basically wood needs to be moisture-free. Wood MUST be dried or kiln-dried to avoid blistering. The best primer would be epoxy. As always, testing is recommended prior to application. The coldest temperature recommended to spray Matthews paint is at 60-65 degrees minimum both inside and outside. Can concrete be painted with Matthews paint? The porosity of the concrete will determine number of coats of epoxy to apply. Concrete should be properly cleaned to remove form release agents. Muriatic acid is best choice for cleaning / etching. Testing is always recommended. How do I get rid of the white spots when I use flattening paste? Stir, shake, and strain Verify proper order of addition of ingredients How can we get Satin MAP to dry more evenly? This can be challenging especially over large, dark, flat surfaces Check equipment setup (1.3-1.5) Try using slower reducer and adding a retarder to the reducer mix Two medium wet coats with second coat applied as a cross coat How can I raise the gloss level of MAP Gloss? Use gloss modifier or gloss clear, this will help achieve a wetter look 2 1-800-323-6593 www.matthewspaint.com

How can I get the paint to dry faster? Bake it, use accelerator, increase air flow, and/or add reducer to assist flash Use proper mix ratios and spray techniques What causes vinyl bubbling? Carbon dioxide from the curing process is trapped by vinyl Allow product to outgas by following proper cure times before applying vinyl Force dry before application Metallic paints present the greatest application challenge. What can I do? Proper technique, equipment setups, film builds Single stage metallic is always tough, needs to be babied on in light coats Gain experience in spraying metallics Basecoat/Clearcoat in place of single stage What are recommendations when paint dries too fast? If due to environment use slower solvent and/or catalyst Otherwise apply wetter, thicker film build What causes paint to bubble, alligator, blister or lift? Incompatible substrate or undercoat Improper catalyzation or improper use of accelerators Topcoated outside cure window Overbaked or baked without purge/flash time What causes paint to chalk? Exposure to sun and elements Under-catalyzation Too thin of film build How long after I paint can I wrap and ship? Depends on sign size, composition/construction, and ambient conditions Best to determine your own window onsite What is the difference between dry and cure times? Dry means out of dust Cure means through dry What happens if I do not put in the proper catalyst? Crosslinking doesn t occur or occurs partially Poor performance will result, lack of long term durability What causes orange peeling? Improper reduction (too little) Improper air pressure (too much or too little) Improper equipment setup (too much fluid, not enough atomization) Any combination of these How many coats do I need? Normally two coats, regardless of number of passes Minimum 2 mil dry film for topcoats The paint doesn t seem to be hiding, what do I do? Use hiding stickers to help determine number of coats Obviously add coats Add stronger basecoat color to get hiding first then topcoat with weaker color Make sure that paint is not over-reduced You can get the paint to dry faster by baking it, using accelerator, increasing air flow, and/or adding reducer to assist flash while using proper mix ratios and spray techniques. 1-800-323-6593 www.matthewspaint.com 3

Paint dries too fast, even with 6396SP Slow Reducer? Add 45-251SP retarder to reducer mix Use 43-999 slow catalyst in place of universal catalyst (43-270SP) What causes blushing? Moisture entrapment (humidity in air gets sucked in as solvent flashes off) Substrates must be at proper temperatures Improper air flow Recoat problems occur when trying to apply additional paint to a freshly painted surface when the original paint film is in its crosslink window. Paint film will lift or wrinkle if additional coats are applied during this window. What are recoat windows and recoat problems? Recoat problems occur when trying to apply additional paint to a freshly painted surface (to repair a defect or for other reasons) when the original paint film is in its crosslink window. That window is an amount of time in which the paint film is still very fresh but not wet, yet not dry enough to resist the solvent from additional coats of paint. Typically a paint film will lift or wrinkle if additional coats are applied during this window. Actual recoat times vary according to film build, technique, application and individual product. Basically speaking, try to apply all of the coats of paint you intend to spray at one time following recommended flash times. If additional coats are necessary later to repair a defect, wait until the paint has dried overnight or force dry it for a comparable time. Troubleshooting Guide This section provides a list of common problems, what causes the problem, and a general list of corrective actions. Orange Peel is a film that has the physical appearance of an orange peel. This is caused when the film lacks ability to flow smoothly. Rough substrate transmits irregularities to subsequent topcoats. Orange Peel Film that has the physical appearance of an orange peel. Cause: Film lacks ability to flow smoothly. Rough substrate transmits irregularities to subsequent topcoats. o Check if defect is on whole unit or in o Check other units on line to determine if pattern exists o Check for low air pressure o Check for under-reduction o Check for proper film build o Check for improper gun distance o Check reducing solvent and viscosity o Check smoothness of substrate o Check if defect is specific to one color o Check for excessive temperature 4 1-800-323-6593 www.matthewspaint.com

Dry Spray A rough, textured surface often confined to a small area. Cause: Paint lacks ability to flow properly. o Check if defect is on whole unit or in o Check if defect is specific to one color or many colors o Check for proper film build o Check for excessive air pressure o Check for improper gun distance o Check reducing solvent selection and spray viscosity Color Match Finished panels do not match color standard. Cause: Variations in application and/or paint materials. o Check other units on-line to determine if a pattern exists o Check for complete hiding o Check for variables in spray application o Check lines and equipment for contamination from previous color o Check for improper mixing o Check for proper agitation o Check gun pattern o Check gun distance o Check equipment setup Sags or Runs Tiers or curtains of paint on vertical or inclined areas. Cause: Paint s inability to uniformly hold to a vertical or inclined surface, producing excessive build-up. o Check other units to determine if a pattern exists o Check if defect is specific to one color or many colors o Check for excessive film build o Check for excessive fluid delivery o Check for improper gun distance (too close) o Check solvent selection (too slow) o Check for insufficient air pressure o Check for excessive application overlap o Check for too short flash time o Check for low spray room temperature o Check temperature of paint o Check temperature of unit o Check for proper reduction Dry Spray is a rough, textured surface usually confined to a small area that is caused by the paint s lack of ability to flow properly. 1-800-323-6593 www.matthewspaint.com 5

Fisheyes Small rounded indentations that resemble fisheyes. Cause: Foreign substances that do not blend with paint. o Check for oil in air lines and spray equipment o Check airborne contamination in spray area o Check for possible contamination in paint materials o Check for painter contamination, skin oils, perspiration, greasy foods, etc. o Check for any oils or contamination that might get into paint or spray area o Check for proper cleaning procedures prior to refinishing Dirt Small bumps deposited in, on, or under the paint film. Cause: Foreign particles entering wet paint film. o Check other units to determine if a pattern exists o Check paint mixing / filtration process o Check spray environment (booth) o Check preparation process of unit, tacking, solvent wash, etc. o Check painter s clothing o Check spray equipment o Check used paint filters for contamination o Check for use of anti-static wipe or spray products Fisheyes are small rounded indentations that resemble fisheyes. This is caused by foreign substances that do not blend with paint. Peeling Topcoat peels off when unmasking. Cause: Topcoat layer or paint separating because of lack of physical bonding. o Check other units to determine if a pattern exists o Check film build wet and dry o Check for contamination oil, sanding residue, overspray, water, cleaner residue, etc. on substrate prior to topcoat application o Check for non-sanding or primer surfacer o Check for case hardening of substrate o Check for poor surface preparation prior to topcoat application o Check for masking tape contacting painted surface o Check solvent selection (too fast) o Check for thin sealer film builds or no sealer o Check for incompatible products 6 1-800-323-6593 www.matthewspaint.com

Soft Paint Easy to mar or penetrate film with fingernail. Cause: Insufficient cure of paint film. o Check other units to determine if a pattern exists o Check for improper film build o Check hardener (old, improper, or contaminated) o Check for improper mixing ratio o Check for improper heat during cure time o Check for improper air flow o Check flash or dry times o Check solvent selection (too fast) o Check for excessive humidity o Check for cool temperatures Die Back Loss of gloss after application (if using glossy topcoat). Cause: Improper evaporation of solvent, poor initial cure, or paint not flattened sufficiently. o Check for too fast a solvent selection o Check for cool temperature during cure o Check for lack of airflow during cure o Check for improper film build o Check for improper flash times o Check for incompatible products o Check for proper mixing/agitation of product Solvent Trap (Popping) A goose pimple or volcano appearance in paint film which, on close examination, frequently has small holes in the center of the bumps. Cause: Improper evaporation of solvent from wet paint film during initial cure or force dry. o Check to determine if defect is on entire unit or just in a o Check for high temperature in first part of force dry o Check other units on line to determine if a pattern exists o Check for correct reducing solvent o Check if defect is specific to one or many colors o Check if defect is most prevalent on horizontal surfaces o Check for excessive film builds o Check for high fluid delivery o Check for low air pressure o Check for high viscosity o Check for too much overlapping in film build Die Back is the loss of gloss after application (if using glossy topcoat). It is caused from improper evaporation of solvent, poor initial cure, or paint not flattened sufficiently. 1-800-323-6593 www.matthewspaint.com 7

Mottling Spotty, non-uniform, blotchy appearance of metallic paint. Cause: Uneven distribution of metallic flakes. o Check if defect is specific to one color or many o Check for excessively high fluid delivery o Check atomizing air pressure o Check gun pattern o Check gun distance o Check equipment set-ups (fluid delivery) o Check solvent selection o Check reduction, viscosity o Check flash and dry times o Check temperature in spray environment (too cool) Sand Scratches & Bullseyes are the objectionable sanding pattern imperfections that show through the finished paint film. They are caused by imperfections due to soft primer, improper sanding techniques and low topcoat film build. Excessive film builds with improper flash times. Sand Scratches & Bullseyes Objectionable sanding pattern imperfections that show through the finished paint film. Cause: Imperfections due to soft primer, improper sanding techniques and low topcoat film build. Excessive film builds with improper flash times. o Check if defect is specific to one or many colors o Check for correct sandpaper grit (too coarse) o Check topcoat film thickness o Check for proper feather edge technique o Check for uncured primer o Check for poor quality solvent used in undercoats o Check flash and dry times o Check for excessive primer film builds o Check for proper gun technique and atomization o Check for under-reduced primer surfacer (bridging scratches) o Check for sanding before primer surfacer is cured Overspray Paint materials from another unit falling on adjacent surfaces. Cause: Misdirected spray droplets or dry spray. o Check to determine if defect is on entire unit or in o Check for correct booth air balance and flow o Check for sequence of panel application o Check gun technique o Check if defect is specific to one color o Check air pressure (too high) o Check for over-reduction 8 1-800-323-6593 www.matthewspaint.com